Synthesis of Zn–Fe double metal cyanide complexes with imidazolium-based ionic liquid cocatalysts via ball milling for copolymerization of CO2 and propylene oxide

Jia Shi a, Zaifeng Shiab, Huiqiong Yana, Xianghui Wanga, Xiaopeng Zhangab, Qiang Lin*abc and Linhua Zhu*abc
aCollege of Chemistry and Chemical Engineering, Hainan Normal University, Haikou, Hainan 571158, P. R. China. E-mail: linqianggroup@163.com; zhulinhua1981@163.com; Fax: +86-0898-65889422; Tel: +86-0898-65889422
bKey Laboratory of Pollution Control of Hainan Province, Hainan Normal University, Haikou, Hainan 571158, P. R. China
cKey Laboratory of Tropical Medicinal Plant Chemistry of Ministry Education, Hainan Normal University, Haikou, Hainan 571158, P. R. China

Received 17th November 2017 , Accepted 22nd January 2018

First published on 9th February 2018


Abstract

In this work, Zn–Fe double metal cyanide (DMC) catalysts were successfully synthesized via clean and efficient ball milling. Imidazolium-based ionic liquids as cocatalysts were incorporated into the structure of the DMC catalysts during the grinding process. The modified Zn–Fe DMC catalysts were effective for the alternating copolymerization of carbon dioxide and propylene oxide under controlled reaction conditions. The properties and structures of the Zn–Fe DMC catalysts and the resulting polymers were characterized by Fourier transform infrared spectroscopy, scanning electron microscopy, X-ray diffraction, elemental analysis, 1H and 13C NMR spectroscopy, gel permeation chromatography, and thermogravimetric analysis. The results indicate that the Zn–Fe DMC catalysts exhibit higher thermal stability compared to the DMC catalysts without imidazolium-based ionic liquids (DMC-Blank). We determined that the introduction of a small amount of imidazolium-based ionic liquids can increase the carbonate content of the poly(propylene carbonate) (PPC) copolymer in the range of 18.48–29.00%. The turnover numbers of PPC were ∼4.40. In addition, the measured number-average relative molecular mass was in the range of 2.96 × 103–4.98 × 103 with a narrow polydispersity index of 1.00–1.08.


Introduction

Carbon dioxide (CO2) is an ideal synthetic C1 resource because it is abundant, renewable, inexpensive, non-toxic and nonflammable.1–5 The utilization of CO2 for the industrial production of aliphatic polycarbonates has attracted significant attention in recent years.6,7 CO2 can be effectively fixed in the copolymerization reaction with epoxides, leading to the synthesis of polycarbonates. Polycarbonates possess outstanding properties: they are highly transparent, durable, biodegradable, and light. As such, they have useful applications in the healthcare, food, and the automotive industries.8–11

It is generally accepted that effective catalysts are critical for the successful synthesis of propylene carbonates from CO2 and epoxides. Since the initial discovery by Inoue and coworkers of the ZnEt2 and water catalyst for the reaction of CO2 and epoxides,12,13 researchers have developed a wide variety of catalytic systems for the synthesis of polycarbonates including zinc carboxylates,14 Salen metal compounds,15 β-diiminate zinc derivatives,16 organic bases,17 metalloporphyrins,18 a rare-earth ternary catalyst,19 organic ammonium halogenides and others.20–23 Among these, double metal cyanide (DMC) catalysts display excellent catalytic activity for the copolymerization of CO2 and epoxides via several different reaction mechanisms.24–27 However, the complicated reaction processes, harsh synthesis conditions, poor activity, and unsatisfactory thermal stability of these catalysts are major drawbacks that urgently need to be addressed. In this regard, the simple and efficient process of mechanochemistry has proven to be effective in activating the copolymerization of CO2 and epoxides.28–31

Catalysts can be synthesized for polycarbonates using a metal complex. They can also be used together with a cocatalyst to enhance their performance in a binary catalyst system. Several different binary catalyst systems have been synthesized for polymerization with good performance.32–34 Ionic liquids (IL) as cocatalysts have unique characteristics which include environmental benignity, thermal and chemical stability, and low volatility compared to conventional organic and inorganic solvents.35–37

In this work, binary catalyst systems of Zn–Fe DMC catalysts were synthesized by the addition of cocatalysts of imidazolium-based ionic liquids (IL) during ball milling. We investigated the properties and structures of the Zn–Fe DMC complexes and the polymers which resulted from the copolymerization of CO2 and propylene oxide (PO) (Scheme 1). The copolymerization of CO2 and PO catalyzed by Zn–Fe DMC complexes with imidazolium-based ionic liquids as cocatalysts, was investigated in this report.


image file: c7ra12528c-s1.tif
Scheme 1 Reaction of CO2 and propylene oxide.

Experimental

Materials

Carbon dioxide (CO2) (purity > 99.9%) and propylene oxide (PO) (≥98%) were used. The chemicals potassium hexacyanoferrate(III) [K3Fe(CN)6], zinc chloride (ZnCl2), 1-butyl-3-methylimidazolium hexafluorophosphate (BMIMPF6), 1-butyl-3-methylimidazolium tetrafluoroborate (BMIMBF4), 1-butyl-3-methylimidazolium bromide (BMIMBr), 1-butyl-3-methylimidazolium chloride (BMIMCl), tert-butyl alcohol (t-BuOH), and trichloromethane (CHCl3) were of analytical purity and used directly without further purification.

Synthesis of Zn–Fe DMC catalysts

The synthesis of the Zn–Fe DMC catalysts was carried out with a planetary ball mill. A mixture of ZnCl2 and K3Fe(CN)6 (molar ratio of 10[thin space (1/6-em)]:[thin space (1/6-em)]1) with 2 mL of t-BuOH was placed separately into five stainless steel vessels. BMIMPF6, BMIMBF4, BMIMBr, and BMIMCl were then added to vessels 2, 3, 4, and 5, respectively, but not to vessel 1. Vessels 1–5 were labelled DMC-Blank, DMC-PF6, DMC-BF4, DMC-Br and DMC-Cl respectively. Subsequently, the mixture was ground at 50 Hz for 10 min. The resulting products were first thoroughly washed with a mixed solution of deionized water and t-BuOH (volume ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]1) to remove excess reactants, then filtered and dried under vacuum at 55 °C.

Copolymerization of CO2 and PO

Copolymerization of CO2 and PO was performed in a 500 mL stainless steel autoclave equipped with a magnetic stirrer, heating water bath, and a check valve. A total of 0.5 g of dried DMC was added to the autoclave, followed by the addition of 30 mL of PO under vacuum conditions. The reactor was then heated to 60 °C and pressurized at 3 MPa with CO2. After 24 h, the autoclave was cooled to room temperature, slowly depressurized, and opened. The resulting products were dissolved in trichloromethane, stirred for 15 min, poured into water, isolated, and dried under vacuum at 55 °C for several hours prior to characterization.

Characterization

The DMC catalysts were characterized using a scanning electron microscope (Model: JEM-7100F), X-ray diffractometer (Bruker AXS/D8), thermogravimetric analyzer at a heating rate of 10 °C min−1 under O2 atmosphere in a high throughput mode (SDT Q600), elemental analyzer (Vario EL Cube), and Fourier transform infrared (FT-IR) spectrometer using KBr tablets (6700/Thermo Fisher Scientific). NMR spectroscopic analyses of the products were performed using a Bruker NMR spectrometer (Model: Bruker AV 400 MHz) with 1H and 13C probes, and CDCl3 as the solvent. The Mn and polydispersity indices (PDI) of the polymer products were estimated using a gel permeation chromatography system.

Results and discussion

Characterization of DMC catalysts

FT-IR spectra of the Zn–Fe DMC catalysts prepared by grinding with various imidazolium-based ionic liquids are shown in Fig. 1. All samples exhibited characteristic absorption peaks which corresponded to those of the Zn–Fe DMC catalysts prepared without ionic liquids (DMC-Blank). For example, the peaks of DMC-PF6 at ∼2100 cm−1 were assigned to the C[triple bond, length as m-dash]N stretching mode of the Zn2+–CN–Fe3+ unit. An absorption peak at 1619 cm−1 could also be clearly observed in the spectra. This stretching vibration corresponded to the weakened C[triple bond, length as m-dash]N bond in the Zn2+–CN–Fe3+ unit, which resembled the C[double bond, length as m-dash]N bond. The weakening of the C[triple bond, length as m-dash]N bond was ascribed to the coordination of Zn2+ with the C[triple bond, length as m-dash]N group. Due to the presence of the complexing agent tert-BuOH, the stretching vibration absorption peaks of the hydroxyl groups appears at 3441 cm−1. In contrast, the peak at 2948 cm−1 was attributed to the C–H stretching vibration absorption and the Fe–CN flexural vibration absorption peaks are located at 600 and 482 cm−1. The C[double bond, length as m-dash]N bond was shifted to higher frequencies compared with DMC-Blank. This indicates that CN acts as a σ-donor by donating electrons to Fe3+, and as a π-electron donor by chelating to Zn2+.38 These FT-IR results also confirm the existence of typical functional groups in the Zn–Fe DMC catalysts.
image file: c7ra12528c-f1.tif
Fig. 1 FTIR spectra of DMC-Blank (a), DMC-PF6 (b), DMC-BF4 (c), DMC-Br (d) and DMC-Cl (e).

The X-ray diffraction (XRD) patterns of the DMC catalysts are depicted in Fig. 2. There are no obvious differences in the crystal patterns of DMC-PF6, DMC-BF4, DMC-Br, DMC-Cl, and DMC-Blank. The observed peaks of the Zn–Fe DMC catalysts are in the range of 2θ = 17.2–24.3° and are of low intensities. However, the reflections at approximately 23.7° (2θ) of the DMC catalyst exhibited a pronounced intensity, which is characteristic of a monoclinic phase with lower phase purity.39,40 It was inferred that the DMC catalysts prepared by ball milling showed high catalytic activity because of their lower crystallinity. Thus, the PO ring could be easily opened, which allows for better penetration of the reactants into the catalyst structure.


image file: c7ra12528c-f2.tif
Fig. 2 XRD patterns of DMC-Blank (a), DMC-PF6 (b), DMC-BF4 (c), DMC-Br (d) and DMC-Cl (e).

An effort was made to examine the morphology and surface shape of the synthesized DMC catalysts using scanning electron microscopy (SEM). As evident from Fig. 3, the SEM images showed that the minimum dimensions of the particles were up to a few hundred nanometers. The physical appearance of the catalysts confirmed the presence of sheet structures and overlapping of the particles with each other. The fragmentation of the Zn–Fe DMC catalysts allowed for an easier introduction of the IL cocatalysts into the catalysts structure. This also resulted in the formation of a high surface area and more activity points for the reactants by the grinding method. As such, a high catalytic activity in the polymerization of CO2 and PO is observed.41


image file: c7ra12528c-f3.tif
Fig. 3 SEM images of the DMC-PF6 (a), DMC-BF4 (b), DMC-Br (c) and DMC-Cl (d).

The elemental composition of the as-prepared Zn–Fe DMC catalysts with various imidazolium-based ionic liquids was determined. The results of these analyses are shown in Table 1. The N and C contents of DMC-PF6, DMC-BF4, DMC-Br, and DMC-Cl are relatively lower than that in DMC-Blank. This result indicate that the ionic liquids are incorporated into the catalysts according to the N and C content, which also shows Zn–Fe DMC catalysts synthesized by ball milling.

Table 1 Elemental composition of the obtained Zn–Fe DMC catalysts in terms of mass fractions
Entry Catalyst IL C (wt%) H (wt%) N (wt%)
1 DMC-Blank 21.99 3.92 16.63
2 DMC-PF6 BMIMPF6 13.69 1.95 12.24
3 DMC-BF4 BMIMBF4 9.21 2.69 8.41
4 DMC-Br BMIMBr 19.18 3.13 13.96
5 DMC-Cl BMIMCl 17.60 3.68 13.35


The thermal stability of the DMC catalysts is an important consideration in the determination of the temperature for activation. The activation temperatures for the synthesized catalysts were investigated by means of thermogravimetric analysis (TGA) and derivative thermogravimetry (DTG) analysis in a N2 atmosphere in a high throughput mode (Table 2 and Fig. 4). The decomposition of DMC catalysts resulted in an initial slight weight loss below 120 °C, which was possibly due to the removal of H2O and t-BuOH from the surface of the catalysts, followed by the loss of IL moieties and cyanide ligands.42 Furthermore, a second significant mass loss was observed in the range of 150–220 °C for the DMC-Blank. This indicated that the catalyst was thermally stable up to ∼250 °C. A total weight loss of 30% was observed for the DMC catalysts with ILs including DMC-PF6 (184 °C) > DMC-BF4 (176 °C) > DMC-Br (175 °C) > DMC-Cl (172 °C) > DMC-Blank (119 °C). Thus, DMC-PF6 is expected to exhibit good stability for catalytic reactions performed at moderately high temperatures.

Table 2 Thermal properties of the DMC catalysts
Entry Catalyst T−5%/°C T−10%/°C T−20%/°C T−30%/°C
1 DMC-Blank 56.84 74.86 157.15 319.21
2 DMC-PF6 109.37 237.84 490.36 658.71
3 DMC-BF4 190.58 261.45 460.78 627.74
4 DMC-Br 118.30 323.58 522.91 664.67
5 DMC-Cl 106.41 299.95 505.23 708.94



image file: c7ra12528c-f4.tif
Fig. 4 TGA (A) and DTG (B) profiles of DMC-Blank (a), DMC-PF6 (b), DMC-BF4 (c), DMC-Br (d) and DMC-Cl (e).

Analysis of copolymer

PPC was synthesized by using the Zn–Fe DMC catalysts for the copolymerization of CO2 and PO. As shown in Fig. 5, for example, the peak of DMC-PF6 at 1772 cm−1 can be assigned to the vibration absorption of C[double bond, length as m-dash]O. The C–O stretching vibration appears at 1205 cm−1. These results demonstrate that an ether backbone was formed in the polymers. Furthermore, the bands that appear at 2926 cm−1 are attributed to the C–H stretching vibrations. Those at 1076 cm−1 were assigned to the C–O–C vibrations. The latter groups were formed as a result of the polymerization of propylene oxide. This confirmed that PPC was successfully obtained by using Zn–Fe DMC catalysts.
image file: c7ra12528c-f5.tif
Fig. 5 FT-IR spectra of PPC-Blank (a), PPC-PF6 (b), PPC-BF4 (c), PPC-Br (d) and PPC-Cl (e).

1H and 13C NMR spectra of the synthesized PPC samples in CDCl3 are shown in Fig. 6(A) and (B), respectively. As evident from Fig. 6(A), three sets of peaks centered at 0.96–1.48 ppm indicate similar H environments in the resultant copolymers, which was assigned to the H of the methyl group. In addition, the two sets of peaks at ∼4.06 ppm are attributed to H having two C–H linkages. The peak at 4.78 ppm indicates the presence of the methylidyne proton. As shown in Fig. 6(B), 13C NMR: δ (ppm) a = 16.5, b = 69.3, c = 71.4, and d = 155.1. This further substantiated the presence of both the carbonate and ether backbone in the resultant copolymers.


image file: c7ra12528c-f6.tif
Fig. 6 1H (A) and 13C (B) NMR spectra of PPC-Blank (a′), PPC-PF6 (b′), PPC-BF4 (c′), PPC-Br (d′) and PPC-Cl (e′).

Copolymerization of CO2 and PO was performed using the same amount of different Zn–Fe DMC catalysts and their catalytic activities are compared (Table 3, entries 1–5). As seen in the table, the DMC-Blank catalyst has the highest number average molecular weight (Mn) (4981) and the lowest content of CO2 (18.48%) (Table 3, entry 1). Among the copolymers produced by the different DMC catalysts, DMC-PF6 was the most active for the copolymerization of CO2 and PO (Table 3, entry 2). The DMC-BF4 catalyst had the highest content of CO2 (29.00%) and PPC (53.85%). These results indicate that imidazolium-based ionic liquids play an important role in enhancing the activity of Zn–Fe DMC catalysts. Scheme 2 depicts the coordination insertion mechanism. The Zn–Fe DMC catalysts showed high catalytic activity because of the assistance of ILs in terms of strong steric hindrance and the electronic environment. From the obtained results and the previously reported data on the interaction energies between the cations and anions employed in this study, the trend of PF6 > BF4 > Br > Cl is observed. This trend is also apparent based on their catalytic activity.43 In particular, PF6 was found to be a highly efficient catalyst for this protocol. The weight losses of the acquired PPC are shown in Fig. 7. It was determined that the decomposition temperature of PPC-PF6 decreased slightly with an increase in thermal stability.

Table 3 Results of PO and CO2 copolymerization with ground DMC as catalystsa
Entry Polymer Catalyst Mn/Mw/PDI TONb Composition (%)c TGA−10%/°C
fCO2 fPO fPC
a Reaction conditions: PO 30 mL, the Zn–Fe DMC complexes 0.5 g, CO2 pressure 3 MPa, 60 °C 24 h.b Turnover number(TON) in g·polymer/g·Zn and turnover frequency in g·polymer/g·Zn h.c Determined by 1H NMR spectra. fCO2 = (A4.78 + A4.06) × 44/(A4.78 + A4.06) × 44 + (A4.78 + A4.06) × 58 + A3.27–3.73 × 58. fPO = (A4.78 + A4.06 + A3.24–3.71)/[2(A4.78 + A4.06) + A3.27–3.73]. fPC = (A4.78 + A4.06)/(A4.78 + A4.06 + A3.27–3.73).
1 PPC-Blank DMC-Blank 4981/5378/1.08 0.53 18.48 76.98 29.89 149.41
2 PPC-PF6 DMC-PF6 3354/3377/1.01 4.40 26.81 67.44 48.28 140.79
3 PPC-BF4 DMC-BF4 2964/2973/1.00 1.20 29.00 65.00 53.85 145.40
4 PPC-Br DMC-Br 3751/3798/1.01 2.53 26.51 67.78 47.54 177.49
5 PPC-Cl DMC-Cl 3584/3631/1.01 1.31 24.74 69.30 43.32 136.07



image file: c7ra12528c-s2.tif
Scheme 2 Proposed structures of the Zn–Fe DMC catalysts.

image file: c7ra12528c-f7.tif
Fig. 7 TGA (A) and DTG (B) profiles of PPC-Blank (a), PPC-PF6 (b), PPC-BF4 (c), PPC-Br (d) and PPC-Cl (e).

Mechanism

Based on experimental findings, the structures of the Zn–Fe DMC catalysts29 and a possible mechanistic pathway of the catalyzed copolymerization reaction are proposed (Scheme 3). The PO monomer initially undergoes ring-opening and is activated by a zinc complex to form the intermediate I.44 The synergistic effect of the iron(III)-cyano-group and the active Zn2+ center in the zinc complex facilitated the insertion of activated CO2 into PO.45,46 We inferred that the nucleophilic anion Y (PF6, BF4, Br, or Cl) of the IL attacked the less sterically hindered carbon atom of the activated epoxide to afford intermediate II. Then the oxygen atom of the ring-opening epoxide attacked CO2 at the central carbon atom to form intermediate III. Thereby, it transfers to the propagating metal polymer chain via intermediate III followed by the facilitation of the activated PO insertion to produce intermediate IV. Cyclic carbonate (PC) was produced accompanied with the loss of Y via intramolecular nucleophilic substitution or cyclization of intermediate III.47,48 Alternating copolymer polycarbonate V was formed by the further insertion of CO2 and the activated PO molecule to ultimately yield the product PPC. The zinc complex and nucleophilic anion Y of the IL work in cooperation with each other, which is essential to enable intramolecular synergistic action in copolymerization. PPC-PF6 exhibited surprisingly high selectivity, likely due to the strong steric hindrance from the coordinated carboxyl groups (when Y = PF6, BF4, Br, or Cl in Scheme 3) and the electron atmosphere.
image file: c7ra12528c-s3.tif
Scheme 3 Proposed mechanism of the alternating copolymerization of PO and CO2 in the presence of the Zn–Fe DMC catalysts with structure III.

Conclusions

Zn–Fe DMC catalytic systems were successfully synthesized by the ball milling method, which is beneficial for the formation of more active sites. Imidazolium-based ionic liquids as cocatalysts were introduced into the structure of catalysts. The modified catalysts exhibited higher catalytic activity for the alternating copolymerization of CO2 and PO. The Zn–Fe DMC catalysts also exhibited good stability during the catalytic reactions performed at moderately high temperatures. It was also determined that the DMC-PF6 catalyst is highly efficient for the copolymerization reaction, while the use of the DMC-BF4 catalyst results in a high content of CO2 (29.00%) and poly(propylene carbonate) (53.85%).

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by the National Natural Science Foundation of China (21766007), the Natural Science Foundation of Hainan (217108), the National Undergraduate Innovation and Scientific Research Projects of China (201711658004), the Innovation and Scientific Research Projects for graduates of Hainan Normal University (Hsyx2016-35), and the Innovation and Scientific Research Projects for graduates of Hainan (Hys2017-143).

Notes and references

  1. Y. S. Qin, X. F. Sheng, S. J. Liu, G. J. Ren, X. H. Wang and F. Wang, J. CO2 Util., 2015, 11, 3–9 CrossRef CAS .
  2. N. von der Assen and A. Bardow, Green Chem., 2014, 16, 3272–3280 RSC .
  3. F. Koschany, D. Schlereth and O. Hinrichsen, Appl. Catal., B, 2016, 181, 504–516 CrossRef CAS .
  4. C. Shi and P. Zhang, Appl. Catal., B, 2015, 170, 43–52 CrossRef .
  5. M. Yu, K. Zhu, Z. Liu, H. Xiao, W. Deng and X. Zhou, Appl. Catal., B, 2014, 148, 177–190 CrossRef .
  6. G. Trott, P. K. Saini and C. K. Williams, Angew. Chem., Int. Ed., 2016, 53, 1607–1610 Search PubMed .
  7. G. P. Wu and D. J. Darensbourg, Macromolecules, 2016, 49, 807–814 CrossRef CAS .
  8. D. Y. Zhang, S. K. Boopathi, N. Hadjichristidis, Y. Gnanou and X. S. Feng, J. Am. Chem. Soc., 2016, 138, 11117–11120 CrossRef CAS PubMed .
  9. S. Kissling, P. T. Altenbuchner, M. W. Lehenmeier, E. Herdtweck, P. Deglmann, U. B. Seemann and B. Rieger, Chem.–Eur. J., 2015, 21, 8148–8157 CrossRef PubMed .
  10. K. Ma, Q. Bai, L. Zhang and B. Liu, RSC Adv., 2016, 6, 48405–48410 RSC .
  11. Y. L. Liu, M. Xiao, S. J. Wang, L. Xia, D. M. Hang, G. F. Cui and Y. Z. Meng, RSC Adv., 2014, 4, 9503–9508 RSC .
  12. S. Inoue, H. Koinuma and T. Tsuruta, J. Polym. Sci., Part B: Polym. Lett., 1969, 7, 287–292 CrossRef CAS .
  13. S. Inoue, M. Kobayashi, H. Koinuma and T. Tsuruta, Macromol. Chem. Phys., 1972, 155, 61–67 CrossRef CAS .
  14. C. Y. Dai, Q. D. Zhu, H. Y. Pang, L. H. Zhu and Q. Lin, Mater. Lett., 2016, 180, 89–92 CrossRef .
  15. M. R. Kember, A. J. P. White and C. K. Williams, Macromolecules, 2010, 43, 2291–2298 CrossRef CAS .
  16. M. Reiter, S. Vagin, A. Kronast, C. Jandl and B. Rieger, Chem. Sci., 2017, 8, 18761882 RSC .
  17. M. Mandal, U. Monkowius and D. Chakraborty, New J. Chem., 2016, 40, 9824–9839 RSC .
  18. R. M. B. Carrilho, L. D. Dias, R. Rivas, M. M. Pereira, C. Claver and A. M. Masdeu-Bultó, Catalysts, 2017, 7, 210–222 CrossRef .
  19. Y. L. Dong, X. H. Wang, X. J. Zhao and F. S. Wang, J. Polym. Sci., Part A: Polym. Chem., 2012, 50, 362–370 CrossRef CAS .
  20. Y. L. Liu, M. Xiao, S. J. Wang, L. Xia, D. M. Hang, G. F. Cui and Y. Z. Meng, RSC Adv., 2014, 4, 9503–9508 RSC .
  21. D. J. Darensbourg and S. J. Wilson, Green Chem., 2012, 14, 2665–2671 RSC .
  22. X. B. Lu and D. J. Darensbourg, Chem. Soc. Rev., 2012, 41, 1462–1484 RSC .
  23. X. B. Lu, W. M. Ren and G. P. Wu, Acc. Chem. Res., 2012, 45, 1721–1735 CrossRef CAS PubMed .
  24. L. J. Jin, H. B. Zeng and A. Ullah, Polym. Chem., 2017, 8, 6431–6442 RSC .
  25. K. Ma, Q. Bai, L. Zhang and B. Y. Liu, RSC Adv., 2016, 6, 48405–48410 RSC .
  26. J. Sebastian and D. Srinivas, Appl. Catal., A, 2014, 482, 300–308 CrossRef CAS .
  27. R. J. Wei, X. H. Zhang, B. Y. Du, Z. Q. Fan and G. R. Qi, Polymer, 2013, 54, 6357–6362 CrossRef CAS .
  28. W. Y. Zhang, L. B. Lu, Y. Cheng, N. Xu, L. S. Pan, Q. Lin and Y. Y. Wang, Green Chem., 2011, 13, 2701–2703 RSC .
  29. W. Y. Zhang, Q. Lin, Y. Cheng, L. B. Lu, B. Lin, L. H. Pan and N. Xu, J. Appl. Polym. Sci., 2012, 123, 977–985 CrossRef CAS .
  30. Z. F. Guo and Q. Lin, J. Mol. Catal. A: Chem., 2014, 390, 63–68 CrossRef CAS .
  31. Z. F. Guo, Q. Lin, X. H. Wang, C. C. Yu, J. Zhao, Y. D. Shao and T. Peng, Mater. Lett., 2014, 124, 184–187 CrossRef CAS .
  32. W. M. Ren, X. Zhang, Y. Liu, J. F. Li, H. Wang and X. B. Lu, Macromolecules, 2010, 43, 1396–1402 CrossRef CAS .
  33. M. S. Liu, K. Q. Gao, L. Liang, J. M. Sun, L. Sheng and M. Arai, Catal. Sci. Technol., 2016, 6, 6406–6416 CAS .
  34. L. Wang, T. F. Huang, C. Chen, J. L. Zhang, H. Y. He and S. J. Zhang, J. CO2 Util., 2016, 14, 61–66 CrossRef CAS .
  35. E. Comin, R. F. de Souza and K. Bernardo-Gusmão, Catal. Today, 2017, 289, 115–120 CrossRef .
  36. M. H. Liu, J. W. Lan, L. Liang, J. M. Sun and M. Arai, J. Catal., 2017, 347, 138–147 CrossRef CAS .
  37. X. Q. Xu, C. G. Wang, H. R. Li, Y. Wang, W. L. Sun and Z. Q. Shen, Polymer, 2007, 48, 3921–3924 CrossRef CAS .
  38. M. M. Dharman, J. Y. Ahn, M. K. Lee, H. L. Shim, K. H. Kim, I. Kima and D. W. Park, Green Chem., 2008, 10, 678–684 RSC .
  39. A. Peeters, P. Valvekens, R. Ameloot, G. Sankar, C. E. A. Kirschhock and D. E. D. Vos, ACS Catal., 2013, 3, 597–607 CrossRef CAS .
  40. A. Peeters, P. Valvekens, F. Vermoortele, R. Ameloot, C. Kirschhock and D. D. Vos, Chem. Commun., 2011, 47, 4114–4116 RSC .
  41. X. H. Zhang, R. J. Wei, X. K. Sun, J. F. Zhang, B. Y. Du, Z. Q. Fan and G. R. Qi, Polymer, 2011, 52, 5494–5502 CrossRef CAS .
  42. D. J. Darensbourg, S. H. Wei, A. D. Yeung and W. C. Ellis, Macromolecules, 2013, 46, 5850–5855 CrossRef CAS .
  43. A. H. Jadhav, G. M. Thorat, K. Lee, A. C. Lim, H. Kang and J. G. Seo, Catal. Today, 2016, 265, 56–67 CrossRef CAS .
  44. X. B. Lu, L. Shi, Y. M. Wang, R. Zhang, Y. J. Zhang, X. J. Peng, Z. C. Zhang and B. Li, J. Am. Chem. Soc., 2006, 128, 1664–1674 CrossRef CAS PubMed .
  45. Y. J. Huang, X. H. Zhang, Z. J. Hua, S. L. Chen and G. R. Qi, Macromol. Chem. Phys., 2010, 211, 1229–1237 CrossRef CAS .
  46. I. K. Lee, J. Y. Ha, C. Cao, D. W. Park, C. S. Ha and I. Kim, Catal. Today, 2009, 148, 389–397 CrossRef CAS .
  47. X. Fu and H. Jing, J. Catal., 2015, 329, 317–324 CrossRef CAS .
  48. X. Li, R. L. Duan, X. Pang, B. Gao, X. H. Wang and X. S. Chen, Appl. Catal., B, 2016, 182, 580–586 CrossRef CAS .

Footnote

Jia Shi and Zaifeng Shi are co-first authors.

This journal is © The Royal Society of Chemistry 2018
Click here to see how this site uses Cookies. View our privacy policy here.