Zhenhua Lin‡
a,
Hai Zhu‡b,
Long Zhoua,
Jianhui Dua,
Chunfu Zhanga,
Qing-Hua Xub,
Jingjing Chang*a,
Jianyong Ouyangc and
Yue Haoa
aState Key Laboratory of Wide Band Gap Semiconductor Technology, Shaanxi Joint Key Laboratory of Graphene, School of Microelectronics, Xidian University, 2 South Taibai Road, Xi'an, China 710071. E-mail: jjingchang@xidian.edu.cn
bDepartment of Chemistry, National University of Singapore, 3 Science Drive 3, Singapore 117543
cDepartment of Materials Science and Engineering, National University of Singapore, 7 Engineering Drive 1, Singapore 117574
First published on 22nd March 2018
The performance of perovskite solar cells (PSCs) including device efficiency and stability is mainly dependent on the perovskite film properties which are critically related to the organic cations used. Herein, we studied the role that the inorganic lithium (Li) cation played in perovskite thin films and its influence on crystal growth, film properties, and device performance. We found that within the threshold limit of a 1.0% molar ratio, the Li dopant had a positive effect on the film formation and properties. However, after replacing more MA+ with Li+, the device performance was degraded significantly with reduced short-circuit current density (Jsc) and fill factor (FF) values. With a doping ratio of 10 mol%, the film morphology, crystallinity, photophysical, and electronic properties totally changed due to the unstable nature of the Li doped, distorted 3-D perovskite structure. The Li doping mechanism was discussed, and it was thought to contain two different doping mechanisms. One is interstitial doping at the much lower doping ratio, and the other is substitutional doping for the MA cation at the higher doping ratio.
The perovskite thin film morphology and properties could be affected by the precursors used, deposition conditions, and post-treatment conditions.20,21 Among them, the precursors used could be well tuned by blending different lead compounds including halide and non-halide compound and organic cations with different ratios. The band gap and electronic properties could be easily tailored by choosing different metal cations like (lead (Pb), tin (Sn)),22–24 different inorganic anions like (bromine (Br), chlorine (Cl)),25–29 and organic ligands like ethylammonium and formamidinium.10,30–33 For example, the Br substituted CH3NH3PbI3 (MAPbI3) exhibited increased band gap and enhanced open-circuit voltage (Voc) in the PSC devices.25–29 The Formamidinium substituted MAPbI3 showed decreased band gap and enhanced light absorption.10,30–33 Moreover, the alkali metal ion (sodium (Na+) or potassium (K+)) dopants could significantly enhance the crystal size and crystallinity, and reduce the charge recombination, resulting in significantly enhanced short-circuit current (Jsc) and PCE.12,34
Previously, lithium (Li) salts have been applied in dye-sensitized solar cells (DSSCs) and lithium–sulfur batteries, and Li ions have been shown to play important roles in power generating in the devices.35–37 Meanwhile, Li salts as doping sources to enhance the hole or electron transport layer conductivity have been reported extensively. It was found that the solar cell performance was enhanced a lot after using Li doped spiro-OMeTAD compound or titanium oxide (TiO2) interlayer in perovskite solar cells.38–40 However, the effect of Li dopant on the perovskite thin film properties as well as the photophysical properties has not been investigated, and it is necessary to understand these mechanisms to achieve high performance perovskite solar cells. In order to investigate the effect on the crystal morphology and charge transport properties, lithium iodine (LiI), or lithium bromide (LiBr) dopants were intentional introduced into the precursors.
In this study, the alkaline metal dopants (LiI, or LiBr) were intentionally incorporated into the CH3NH3PbI3 precursor solution prior to the thin film formation. Different molar ratios of LiI or LiBr were introduced into the precursor solutions with respect to the PbI2. We investigated the lithium dopant effect on the perovskite thin film formation, absorption, charge transport, and photovoltaic properties. It was found that proper amount of lithium dopant can significantly alter the optical properties and enhance Voc. Meantime, the Jsc showed slightly increase firstly and then sharp decrease when gradually increasing the Li content. Unlike the DSSC devices, it was found that the excess Li ion can enhance the charge carrier density, which is desirable for high performance device.
The thin film absorption spectra with different LiI and LiBr ratios were shown in Fig. 1c and d. The MAPbI3 thin film had strong absorption from the visible range down to the near-infrared wavelengths with the absorption onset at ca. 780–785 nm (optical band gap = 1.58 eV). The measured shape was consistent with the literature reported results.20 The long absorption onset showed slightly blue-shift for the Li doped films compared to the pristine CH3NH3PbI3 thin film. The band gap determined by the onset was about ∼1.61–1.62 eV for 0.5–5.0 mol% LiBr doped thin film, and it showed a 0.01–0.02 eV blue-shift compared to the pristine perovskite.
This tread could be explained by the doping mechanism. When the Li doping ratio was small, the Li ion mainly adopted interstitial doping since the Li ion (76 pm) is much smaller than MA cation (119 pm).12 In this case, the Li ion did not occupy the MA position but only occupied the empty site and enhanced the carrier density, resulting in slightly decreased band gap may be due to the impurity band caused by the Li doping and orbital coupling with neighbor Pb–I orbitals (Fig. S3†). When the Li doping ratio increased above 5 mol%, the excess Li ions would substitute the MA cations, and cause the crystal structure distortion. According to the density functional theory (DFT) calculation results, the fully Li substituted perovskite thin film showed a large band gap of around 1.79 eV which was much larger compared to MA based perovskite thin film.41 Then, the band gap increased again (Fig. S3†). However, in the 3D perovskite structure, when doping with some elements or functional groups with larger or smaller ionic radius, the crystal structure usually has the distortions. In this case, a semi-empirical approach based on the Goldschmidt tolerance factor τ is employed to evaluate the stability of the structure. It is known empirically that 3D perovskite should form when the tolerance factor falls within a narrower range τ = 0.7–1.1. And according to the DFT calculation in the literature, the Li cation doping produces a tolerance factor below 0.7, which makes it unstable towards stable 3D perovskite structure.41
The perovskite thin film morphology was further investigated by field-emission scanning electron microscopy (FESEM). As shown in Fig. 2, the prepared thin films with different Li doping ratios showed much uniform and full surface coverage with regular crystallites. The good thin film uniformity and coverage suggested a homogenous nucleation on the PEDOT:PSS surface due to the proper control on the crystal formation and growth. SEM images showed the corresponding morphology evolution of perovskite films upon changing the Li ratio. The pristine film was compact and conformal. It seemed that the films could tolerate the Li+ ions to the precursor up to around 3.0 mol% before any obvious morphology change occurred, and the film still kept compact and uniform. This is consistent with the XRD results. However, when the ratio increased to 5.0 mol%, some newly formed phase crystals appeared between the MAPbI3 grains, and the morphology changed. When the Li ratio further increased to 10.0 mol%, the large nanoplate-like regular crystals were formed on the substrates, indicating a different crystal behavior upon adding the Li ions. It was thought that the Li cations enhanced the MAPbI3 crystallization, reduced the nucleation density and favored a homogeneous nucleation on the substrates. However, it also produced proper pinholes between the crystal grains which are harmful for the solar cell device performance due to increased charge recombination and leakage. Compared to LiI based thin films, it was found that the crystal morphology was more uniform after Br substitution occurred. Previously, it has been reported that, the Br ion could enhance the thin film properties due to retarded crystallization. Fig. 2(l) shows the cross-section SEM image of perovskite device based on 0.5 mol% LiI doped perovskite, and a dense and uniform perovskite layer could be identified. Moreover, the perovskite crystals were direct contact with PEDOT:PSS and PCBM layers, indicating a high quality of the perovskite film, which could contribute to enhancing the photovoltaic performance.
Fig. 2 (a)–(k) Top-view SEM images of perovskite thin films based different ratios of Li doping. (l) Cross-section image of perovskite device based on 0.5 mol% LiI doped perovskite. |
The planar heterojunction device structure with a configuration of ITO/PEDOT:PSS/perovskite/PCBM/BCP/Ag was used. Current density (J)–voltage (V) characteristics of the device fabricated with the same film formation condition has been shown in Fig. 3. The Voc, Jsc, fill factor (FF), and PCE of all devices are summarized in Table 1. As can been seen, the Li incorporation had a large influence on the device performance. The device exhibited a comparable efficiency of 13.1% for pristine thin film with Jsc, Voc, and FF of 19.6 mA cm−2, 0.93 V, and 0.72, respectively. The 0.5 mol% LiI doped MAPbI3 showed slight increase in PCEs due to enhanced Jsc and Voc, indicating that the impurity threshold limit of the films was 0.5% molar ratio. The corresponding Jsc, Voc, FF and PCE were 20.1 mA cm−2, 0.97 V, 0.73, and 14.2%, respectively. When the doping ratio increased to and 1.0 mol%, and even up to 5 mol%, Jsc and FF gradually reduced. The resulting PCE also decreased to 13.0%, 8.7% and 5.4% for 1%, 3% and 5% molar ratio doped film, respectively. The lower Jsc and FF indicated a high series resistance (Rs) and large charge recombination in the device, which may be due to Li-induced charge traps in the thin film that quenched the photo-generated charge carriers. The PCE of MAPbI3 devices further decreased to 4.8% for the devices with 10% molar doping ratio of samples. And the decrement of PCE was reflected by a reduction of Voc due to structure change induced by the Li impurities. The Jsc, Voc, and FF were 10.5 mA cm−2, 0.96 V, and 0.48, respectively.
Fig. 3 J–V characteristics of different LiI (a) and LiBr (b) doped perovskite thin film devices. IPCE spectra of perovskite solar cells based on different LiI (c) and LiBr (d) dopants. |
Conditions | Jsc (mA cm−2) | Voc (V) | FF | PCE (%) | Rs (Ω cm2) |
---|---|---|---|---|---|
PbI2, control | 19.6 ± 0.2 | 0.94 ± 0.02 | 0.73 ± 0.02 | 13.1 ± 0.5 | 3.66 |
LiI (0.25 mol%) | 19.8 ± 0.2 | 0.95 ± 0.02 | 0.74 ± 0.02 | 13.8 ± 0.4 | 2.88 |
LiI (0.5 mol%) | 20.1 ± 0.2 | 0.97 ± 0.02 | 0.74 ± 0.02 | 14.3 ± 0.4 | 2.09 |
LiI (1.0 mol%) | 18.4 ± 0.2 | 0.98 ± 0.02 | 0.73 ± 0.02 | 13.0 ± 0.4 | 2.25 |
LiI (3.0 mol%) | 13.4 ± 0.3 | 1.03 ± 0.03 | 0.65 ± 0.03 | 8.7 ± 0.6 | 2.47 |
LiI (5.0 mol%) | 9.9 ± 0.4 | 1.04 ± 0.03 | 0.51 ± 0.04 | 5.4 ± 0.8 | 2.74 |
LiI (10.0 mol%) | 10.5 ± 0.5 | 0.96 ± 0.04 | 0.50 ± 0.06 | 4.8 ± 0.9 | 3.97 |
LiBr (0.5 mol%) | 20.3 ± 0.2 | 0.97 ± 0.02 | 0.73 ± 0.02 | 14.1 ± 0.3 | 2.13 |
LiBr (1.0 mol%) | 18.8 ± 0.2 | 0.98 ± 0.02 | 0.74 ± 0.02 | 13.5 ± 0.4 | 2.48 |
LiBr (3.0 mol%) | 14.6 ± 0.3 | 1.03 ± 0.02 | 0.68 ± 0.02 | 9.9 ± 0.6 | 2.94 |
LiBr (5.0 mol%) | 10.8 ± 0.4 | 1.05 ± 0.03 | 0.60 ± 0.04 | 5.3 ± 0.7 | 3.69 |
LiBr (10.0 mol%) | 13.9 ± 0.4 | 0.95 ± 0.04 | 0.49 ± 0.05 | 6.2 ± 0.8 | 4.76 |
It is believed that proper Br doping could stabilize the Li doped perovskite, probably due to its decreased atomic radius of Br compared to I, which can reduce the crystal strain, and hence, the stability was enhanced. The beneficial role of Br doping provides a practical approach to further enhance the device performance of PSCs. For LiBr case, the 0.5 mol% doped perovskite thin film enhanced the Jsc and Voc to 20.3 mA cm−2 and 0.97 V, respectively. Hence, the resulting PCE was enhanced to 14.1%. Further increasing the LiBr doping ratio, the Jsc decreased from 19.6 mA cm−2 for MAPbI3 to 18.8 mA cm−2, 14.6 mA cm−2, 10.8 mA cm−2, 13.9 mA cm−2 for Li with a molar ratio of 1%, 3%, 5%, and 10%, respectively. The Voc increased from 0.93 V for MAPbI3 to 0.98 V, 1.03 V, 1.05 V, and 0.95 V for Li with a molar ratio of 1%, 3%, 5%, and 10% molar ratio, respectively. The FF decreased to 0.66, 0.58, 0.47 for 3%, 5%, and 10% molar ratio, respectively, due to increased leakage current and charge recombination. The resulting PCE values were 13.5% (1.0 mol%), 9.9% (3 mol%), 5.3% (5 mol%), and 6.2% (10 mol%), respectively. Compared to LiI dopant, the devices with LiBr dopant exhibited higher Jsc which might be ascribed to the improved charge carrier transport and reduced charge recombination induced by impurities-related traps. In order to understand the Li doping effect on the photovoltaic performance of the PSCs, the Rs of the devices was obtained from the J–V curves. The Rs was 3.66 Ω cm2 for the pristine perovskite film based device. It decreased to 2.09 Ω cm2 and 2.13 Ω cm2 for the devices with 0.5 mol% LiI and LiBr doped CH3NH3PbI3, respectively. The steady-state PCE outputs at the maximum power point as a function of time were also checked. As shown in Fig. S4,† the stabilized PCEs were 13.2%, 14.3%, and 14.5% for pristine, 0.5 mol% LiI, and 0.5 mol% LiBr doped perovskite, respectively. This indicates that the device results are stable and reliable.
The effect of Li incorporation was also tested by internal photo-electron conversion efficiency (IPCE) measurements. It is known that the IPCE spectra could provide the information on the components primarily responsible for converting absorbed photos to the collected electrons and holes. As shown in Fig. 3c and d, it could be observed that proper Li amount could enhance the IPCE. The integrated Jsc were 19.8 mA cm−2 and 20.5 mA cm−2 for 0.5 mol% LiI and LiBr doped perovskite device, respectively. When the Li doping ratio increased to above 1.0 mol%, the intensity decreased a lot due to the reduced conversion efficiency. This is slightly different from the observed absorption spectra which showed similar absorption for both thin films due to relatively small change in the absorption spectra by this small amount of Li doping.
In order to further elucidate the Li doping effect on the electronic structure of the MAPbI3, UPS measurement was performed on the pristine perovskite and 10% molar ratio of Li doped perovskite composite. The UPS energy levels have been shown in Fig. 4. The secondary electron cutoff of the pristine perovskite film prepared on ITO substrate was located at 17.1 eV, and the valence band maximum was located at 1.6 eV. Since the energy band of the perovskite was about 1.58 eV, it can be concluded that the Fermi level lay close to conduction band edge of the perovskite, indicating an n-type characteristics of the perovskite material. After incorporating Li into the perovskite structure, the secondary electron cutoff slightly shifted by 0.32 eV and 0.38 eV towards the higher binding energy region, indicating an upshift of the Fermi level of about 0.32 eV and 0.38 eV for 10 mol% LiI and 10 mol% LiBr, respectively. The large Fermi level shift indicated an increased electron density for the Li doped MAPbI3. And this low performance might be due to the poor junction between MA1−xLixPbI3 and PCBM in the solar cell device. Anyway, we achieved a highly n-doped perovskite MA1−xLixPbI3, and applied it in the perovskite solar cell. And it is expected that the solar cell efficiency could be further improved by choosing spiro/MA1−xLixPbI3 system due to favorable energy level alignment.
To investigate the photophysical process associated with the Li in the perovskite phase, steady-state photoluminescence (PL) and time-resolved PL measurements were carried out on these thin films. From the steady-state PL, it could be observed that the Li incorporation slightly increased the PL intensity. Time-resolved PL was performed to probe the carrier lifetime of perovskite films prepared on glass substrates. Detailed information about the samples preparation, measurement, and fitting methodology can be found in the experimental part. The PL lifetime of the samples was fitted with a bi-exponential decay function which included a fast decay and a slow decay process. Generally, the radiative electron–hole recombination occurs by two different pathways with two different time scales contributing to the PL decay curves. The PL decay spectra of the samples are shown in Fig. 5b, and the related parameters are summarized in Table 2. The fast decay lifetimes of the pristine perovskite film, 10 mol% LiI doped perovskite film and 10 mol% LiBr doped perovskite film were 1.93 ns, 3.5 ns and 5.0 ns, respectively, and the corresponding slow decay lifetimes of these three samples were 7.74 ns, 21.0 ns, and 31.8 ns, respectively. We have observed a larger PL yield and slower carrier lifetime in the Li doped samples, indicating a decreased nonradiative decay rate, which was likely due to a reduced defect density that suppressed nonradiative recombination.
Fig. 5 Steady-state PL and time-resolved PL spectra for pristine and Li doped perovskite thin films on glass substrates. |
Fraction 1 | τ1 (ns) | Fraction 2 | τ2 (ns) | τave (ns) | |
---|---|---|---|---|---|
0% | 0.47 | 1.93 | 0.53 | 7.74 | 6.68 |
10% LiI | 0.61 | 3.5 | 0.39 | 21.0 | 17.34 |
10% LiBr | 0.73 | 5.0 | 0.27 | 31.8 | 23.73 |
These results can be further supported by femtosecond transient absorption spectroscopy and pump–probe measurements. Femtosecond transient absorption spectroscopy was performed to study the electron dynamics under excitation of femtosecond laser pulses with wavelength centered at 500 nm, pulse duration of 100 fs and repetition rate of 500 Hz. Fig. 6a–c showed the transient absorption spectra of each films at different time delays. The transient absorption spectra of different perovskite films displayed similar profiles with two major features, a transient bleaching band and a photo-induced absorption band, indicating depopulating of the ground state and the presence of charge carriers. The LiBr doped perovskite film exhibited the highest transient bleaching intensity compared to the other two counterparts, while the pristine perovskite film showed the lowest intensity, which was consistent with the steady-state and time-resolved PL measurements, as the transient bleaching signal originated from the stimulated emission of the samples.
To monitor the evolution of the carriers upon optical excitation, the single wavelength dynamics probed at 720 nm were shown in Fig. 6d, giving a carrier lifetime of 176 ± 4 ps, 205 ± 8 ps and 305 ± 10 ps for pristine perovskite film, LiI doped perovskite film, and LiBr doped perovskite film, respectively. The presence of excess Li dopants led to rapid charge recombination, as evidenced by the rapid decay of the pristine perovskite film. While 10 mol% LiI or LiBr doped perovskite film could reduce the amount of charge recombination at long timescales. The results of transient absorption spectroscopy and pump–probe measurements provided further support for the results and discussion in the previous sections.
Footnotes |
† Electronic supplementary information (ESI) available: XRD spectra, band gap of doped perovskite, steady-state PCE output. See DOI: 10.1039/c8ra01199k |
‡ These authors contributed equally to this work. |
This journal is © The Royal Society of Chemistry 2018 |