Qidong Wang,
Taka-Aki Asoh and
Hiroshi Uyama*
Department of Applied Chemistry, Graduate School of Engineering, Osaka University, 2-1 Yamadaoka, Suita, Osaka 565-0871, Japan. E-mail: uyama@chem.eng.osaka-u.ac.jp
First published on 3rd April 2018
This study deals with the unique morphology and properties of methylene diphenyl diisocyanate (MDI)-modified bacterial cellulose/poly(N-isopropylacrylamide) (BC/PNIPAAm) composite hydrogel prepared by in situ polymerization method. The influence of the molar ratio of MDI/glucose unit of BC on the properties of the resulting hydrogel was investigated. Scanning electron microscopic analysis revealed that after the MDI modification the BC/PNIPAAm hydrogel could preserve the unique layered (known as anisotropic) structure. The mechanical property evaluated by stress–strain test was significantly enhanced when compared to that of neat PNIPAAm hydrogel, due to the presence of the BC matrix as well as the MDI modification. Based on the deswelling behaviors, the BC/PNIPAAm hydrogel exhibited improved and controlled responsive rate when compared with neat PNIPAAm hydrogel. Furthermore, the anisotropic thermo-sensitive property was proved by temperature-responsive test with the fact that the composite hydrogel could only deswell and swell in the axial perpendicular to the layers. Along with desired recyclability, the present composite hydrogel may have an application as artificial muscles.
Poly(N-isopropylacrylamide) (PNIPAAm) is one of the most investigated polymers for preparing hydrogel actuators. It undergoes reversible lower critical solution temperature (LCST) phase transition from a swollen hydrated state to a shrunken dehydrated state, which is the result of the competition between the hydrophilic amide and hydrophobic isopropyl moieties in the polymer side-chain.5–7 LCST of PNIPAAm hydrogel is close to body temperature and relatively insensitive to other environmental conditions such as pH and light, which makes PNIPAAm suitable for biomedical application.8 Previously, anisotropic movement of PNIPAAm-based hydrogels has been successfully achieved.9–13 However, the volume changes of the PNIPAAm hydrogels are known to proceed very slowly,14,15 which indicates unsatisfactory responsive rate. Fast actuation in response to temperature change is often important for smart hydrogels. Furthermore, like other hydrogels, common PNIPAAm hydrogels possess poor mechanical properties.
Bacterial cellulose (BC) is a promising candidate as polymer matrix to enhance PNIPAAm hydrogels. Compared to widely used plant-derived cellulose, BC enjoys its distinguishing advantages such as high purity, high porosity and high water content.16–18 Along with good biodegradability and biocompatibility, BC becomes an ideal choice in biomedical and biotechnological fields. It's potential applications are wound dressing, tissue regeneration, skin substitutes19–22 and drug delivery system.23,24 The high crystallinity of BC results in excellent mechanical strength of high Young's modulus, tensile and compressive strength,25,26 making it act as ideal reinforcing element in polymer matrix. Moreover, BC with layered structure can be prepared by static culture of certain bacteria.25,27 This kind of anisotropic structure brings about mechanical anisotropy to BC.28 In spite of these outstanding features, pristine BC lacks certain functions and properties (i.e., stimuli–responsive property), which limits its applications in various fields. Therefore, synthesis of BC composites has been conducted to address these limitations. Many researchers focus on the preparation of BC-based functional composites with other polymers or inorganic materials to enlarge the potential applications of BC.29–31
In this study, in order to overcome the shortcomings of BC and PNIPAAm hydrogels, a 4,4′-methylenediphenyl diisocyanate (MDI)-modified BC/PNIPAAm composite hydrogel was prepared by a simple in situ polymerization method. With the layered structure, the composite hydrogel would show the desired anisotropic thermo-sensitivity (Fig. 1). The morphological, thermal and mechanical properties of the resultant product was investigated by scanning electron microscopy (SEM), differential scanning calorimetry (DSC), and compressive stress–strain measurements to reveal their structure, LCST behavior and physical strength. The temperature dependences of the swelling ratio and deswelling behaviors of the hydrogel were characterized. In particular, the size changes of the hydrogel in three dimensions were carefully studied to confirm the anisotropic thermo-sensitivity of the present composite hydrogel. By the combination of MDI-modified BC and PNIPAAm, the composite hydrogel is aimed to have uniaxial deswelling–swelling (so-called anisotropic thermo-sensitivity), enhanced mechanical strength as well as fast response rate to temperature change.
Fig. 1 Schematic illustration of complex formation of MDI-BC/PNIPAAm and uniaxial deswelling above LCST. |
Swelling ratio = (Ws − Wd)/Wd | (1) |
The deswelling behaviors of the hydrogel were studied at 50 °C (above LCST) gravimetrically. At regular time intervals, the samples were taken out and weighed after removing the excess water. Water retention is defined as follows:
Water retention = [(Wt − Wd)/(We − Wd)] × 100 | (2) |
For the anisotropic thermo-sensitive property, the samples were immersed in water at 50 °C. l/l0 and w/w0 were shrinking (or deswelling) ratios parallel to the layer structure of BC/PNIPAAm hydrogel, and t/t0 was that perpendicular, where l0, w0, t0 were the length, width and thickness of the gel samples at equilibrium state in 20 °C solution and l, w, t were those at determined time at 50 °C in water solution. The length, width and thickness of the hydrogel samples were measured by a caliper.
COM0 | COM1 | COM2 | COM3 | |
---|---|---|---|---|
a Dry weights of BC in all the samples were 17 mg. | ||||
MDI-BC (mg) | — | 22 | 43 | 64 |
MDI:glucose unit of BC (mol:mol) | — | 0.19:1 | 0.98:1 | 1.77:1 |
BC/PNIPAAm or MDI-BC/PNIPAAm (mg) | 160 | 161 | 161 | 161 |
Weight ratio of PNIPAAm (wt%) | 89% | 86% | 73% | 60% |
MDI-modified BC/PNIPAAm composite hydrogels were also studied by FT-IR spectra (Fig. S1†). Despite the difference in the MDI/glucose unit molar ratios, all the samples showed very similar FT-IR spectra. A sharp absorption peak at 3300 cm−1 is assigned to hydroxyl groups of BC. The samples had peaks at 1640 and 1540 cm−1 which are referred to the amide I and amide II of PNIPAAm, respectively. Notice that there was no obvious difference between the spectrum of COM0 hydrogel and those of COM1, COM2, COM3. This is probably due to the reason that the IR spectrum of the urethane group derived from MDI is similar to that of PNIPAAm with the amide group.
According to the SEM images of pure BC hydrogel (Fig. 2a and b), the 3D network structure of BC was confirmed in the horizontal image while it showed an excellent layered structure in the vertical direction, indicating the anisotropic structure of BC. However, the BC/PNIPAAm hydrogel (COM0) lost this layered structure (Fig. 2d), resulting in porous morphology. When BC was cross-linked by MDI before the polymerization of PNIPAAm, the layered structure in the vertical direction could preserve to some extent (Fig. 2f, h and j) while the horizontal images displayed the 3D network structure. The more the MDI ratio, the better the layered structure inside the hydrogel remained. Thus the average thickness of the layers decreased with increasing the MDI ratio and the average thickness of COM3 was close to that of pure BC. The SEM observation indicates that the anisotropic composite hydrogels were successfully prepared. This unique structure was believed to endow special properties to the hydrogels, which would be mentioned below.
Fig. 3 shows the stress–strain curves of the composite hydrogels including pure BC in the vertical direction (perpendicular to the layered structure), whereas data obtained from these tests can also be found in Table 2. The data prove that the introduction of BC and MDI-modified BC would greatly improve the mechanical property of PNIPAAm hydrogel. The maximum compressive strength of COM0 was 532 kPa whereas that of PNIPAAm hydrogel was 20 kPa. With the increase of the MDI/glucose unit ratio, the compressive strength increased gradually. COM3 had the largest compressive strength of 838 kPa, which was about 40 times of that of the PNIPAAm hydrogel. This significant improvement of mechanical strength is believed to be beneficial to various applications. The SEM images show that the composite hydrogel with the higher MDI/glucose unit ratio has the smaller layer thickness, making the sample more rigid. As a result, the MDI-modified BC/PNIPAAm hydrogel with the higher MDI/glucose unit ratio would have better mechanical strength.
Fig. 3 Stress–strain curves of BC/PNIPAAm composite hydrogels with different MDI ratio, BC and PNIPAAm hydrogels under compression. |
Sample | Compressive strength (kPa) | Strain at break (%) |
---|---|---|
BC | 938 | 89 |
COM0 | 532 | 72 |
COM1 | 682 | 36 |
COM2 | 770 | 41 |
COM3 | 838 | 50 |
PNIPAAm | 20 | 77 |
The LCST of the series of the hydrogel samples were examined by DSC (Fig. S2†). The onset temperature of endotherm was referred as LCST. Obviously, all the samples showed almost the same LCST at about 32 °C, which matched well with the LCST of PNIPAAm hydrogel. From these data, the BC or MDI-modified BC hydrogel was found to have little impact on LCST of PNIPAAm, indicating that the networks of BC (or MDI-BC) and PNIPAAm are chemically identical and no reaction occurred between them. It is well known that LCST is the point where the hydrophobic interaction of the isopropyl group of PNIPAAm outweighs the hydrophilic nature of the amide group in the pendant group, forcing water out of the hydrogel.35 The subsequent research and applications are mainly based on this LCST of the composite hydrogel.
The temperature dependence of ESR is shown in Fig. 4. The swelling data here showed that all the samples had similar classical thermo-responsive profile. The ESR of all the hydrogels decreased dramatically toward their LCST and had the sharpest decrease around 32 °C where the phase separation occurred. Above the LCST, the hydrogel samples showed almost the same level of ESR regardless of the MDI ratio difference. The LCST from the ESR observation is in good agreement with the thermal data of the DSC study.
Fig. 5 exhibits the deswelling behaviors of the composite hydrogels in water at 50 °C (above LCST). After 20 h, all the five hydrogels including PNIPAAm had a similar water retention of around 3–4% (data not shown in Fig. 5). However, the composite hydrogels showed the relatively faster response to this temperature in the initial 60 min, i.e., COM3 lost about 40% water in the first 10 min whereas pure PNIPAAm hydrogel only lost less than 15% water in the same time period. About 76% water was freed from COM3 in 30 min whereas PNIPAAm showed only 43% water release in the same time frame. The order of water lose rate within 30 min was COM3 > COM2 > COM1 > COM0 > PNIPAAm. The composition between BC and PNIPAAm as well as the MDI modification significantly improved the responsive rate of the hydrogel. Generally, PNIPAAm-based hydrogels present slow responding property to temperature. For example, Okano et al. reported that only 15% volume shrinkage was observed for a PNIPAAm-based hydrogel disk for 60 min on heating from 10 to 40 °C.14 Up to now, three main kinds of strategies have been developed to improve the response rate of PNIPAAm-based hydrogels as follows: (1) diminishing the dimension of hydrogels, (2) generating porous structures of hydrogels, and (3) chemically modifying polymeric networks of hydrogels.36 In our case, the size of PNIPAAm gel in the BC/PNIPAAm composite was reduced mainly due to the layered BC matrix, leading to the rapid response to temperature change. On the other hand, the PNIPAAm-based hydrogels usually form dense hydrophobic layers on outmost surface – so-called skin layers above LCST,37 which results in slow volume change. BC with high hydrophilicity in the BC/PNIPAAm composite hydrogels may inhibit the formation of the skin layers, which would induce the increase in the response rate of the composite hydrogel.
Commonly, PNIPAAm-based hydrogels have a homogeneous structure, resulting in an isotropic thermo-sensitive property. On the other hand, the anisotropic structure of the present MDI-modified BC/PNIPAAm hydrogels as shown in the SEM images influences the thermo-sensitivity. As shown in Fig. 6a, COM3 clearly exhibited the uniaxial deswelling behavior in response to temperature change. The thickness of the hydrogel decreased gradually whereas the length and width remained almost unchanged. The photos of uniaxial deswelling of COM3 above LCST are shown in Fig. 6b. The equilibrium deswelling of the hydrogels with different MDI ratios above the LCST is concluded in Fig. 6c. In the direction perpendicular to the layered structure (vertical), COM0, COM1, COM2 and COM3 shared a similar thickness deswelling ratio (t/t0) of about 20%. However, the deswelling ratio parallel to the layered structure (horizontal) gave the different result: l/l0 and w/w0 of COM0 were less than 80% whereas those of COM1, COM2 and COM3 were more than 95%. In the present composite hydrogel, the PNIPAAm network could swell freely only in the direction perpendicular to the BC layers whereas in other two directions (parallel to the layers), the swelling was almost completely restricted by the rigid BC layers, resulting in the uniaxial deswelling–swelling. Once deswelling above LCST, the BC/PNIPAAm gel could swell back to its original hydrogel state below LCST. This process was reversible and easily controlled by temperature change. The SEM images of the dried composite gel (COM3) were shown in Fig. S3.† Visibly, the BC fibrils arranged randomly in the horizontal direction whereas in the vertical direction the sample showed the excellent layered structure. Therefore, the BC fibrils in the dried composite gel are arranged in an anisotropic manner. Fig. 6d shows the repeatable swelling behavior of dried COM3 below or above LCST. It hardly absorbed any water at 50 °C because PNIPAAm showed hydrophobicity above LCST. However, at 20 °C the dried COM3 swelled well and absorbed a large amount of water (>1000% of the dried gel weight) to recover back to its original hydrogel state. Moreover, the water uptake ability of COM3 almost remained unchanged below or above LCST after many cycles, indicating the desired recyclability of the present composite hydrogel.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8ra01639a |
This journal is © The Royal Society of Chemistry 2018 |