Hyunseock Jieab,
Wenbin Qiua,
Daniel Gajdac,
Jeonghun Kimd,
Valiyaparambil Abdulsalam Anvarae,
Arend Nijhuise,
Yoshio Bandoaf,
Yusuke Yamauchi*dg,
Vladimir Luzin*b and
Md. Shahriar A. Hossain*ah
aAustralian Institute for Innovative Materials (AIIM), University of Wollongong, Squires Way, North Wollongong, NSW 2500, Australia. E-mail: shahriar@uow.edu.au
bAustralian Nuclear Science & Technology Organisation (ANSTO), Lucas Heights, NSW 2232, Australia. E-mail: vll@ansto.gov.au
cInstitute of Low Temperature and Structure Research Polish Academy of Sciences, ul. Okólna 2, 50-422 Wrocław, Poland
dSchool of Chemical Engineering, Australian Institute for Bioengineering and Nanotechnology (AIBN), The University of Queensland, Brisbane, QLD 4072, Australia. E-mail: y.yamauchi@uq.edu.au
eThe University of Twente, Faculty of Science & Technology, 7522 NB Enschede, Netherlands
fInternational Center for Materials Nanoarchitectonics (WPI-MANA), National Institute for Materials Science (NIMS), 1-1 Namiki, Tsukuba, Ibaraki 305-0044, Japan
gDepartment of Plant & Environmental New Resources, Kyung Hee University, 1732 Deogyeong-daero, Giheung-gu, Yongin-si, Gyeonggi-do 446-701, South Korea
hSchool of Mechanical and Mining Engineering, The University of Queensland, Brisbane, QLD 4072, Australia
First published on 26th November 2018
Magnesium diboride (MgB2) superconducting wires have demonstrated commercial potential to replace niobium–titanium (NbTi) in terms of comparable critical current density. Its higher critical temperature makes MgB2 wire suitable for liquid-helium-free operation. We recently reported boron-11 isotope-based low-activation Mg11B2 superconducting wire with decent critical current density appropriate for low-cost superconducting fusion magnets. In this study, we have mainly focused on the neutron diffraction technique to measure the residual stress in Mg11B2 superconducting wire for the first time. The residual stress state was given qualitative and quantitative interpretation in terms of micro- and macrostress generation mechanisms based on the isotropic model confirmed by neutron texture measurements. The relationship between the stress/strain state in the wire and the transport critical current density is also discussed. This investigation could pave the way to further enhancement of the critical current density of low-activation Mg11B2 superconducting wires suitable for next-generation fusion grade magnets.
The critical point in reactor application is the use of boron-11 isotope enriched powder for the fabrication of the MgB2 superconductor. Natural boron has 19.78 wt% boron-10 (10B) and 80.22 wt% boron-11 (11B).16–18 10B is well known as a neutron absorption material with a large nuclear reaction cross-section, leading to transformation into 7Li and He via the (n, α) reaction.19–21 In contrast, 11B is stable in the presence of neutron irradiation without an (n, α) reaction and can reduce nuclear heating.22,23 Therefore, 11B isotope based Mg11B2 superconductor is the most desirable, if not absolutely necessary, material for Tokamak type magnets in fusion reactors.
In recent ITER superconducting cable performance tests, damage to the superconducting filaments has been recognised as a significant issue.24 It was demonstrated that the superconducting filaments in the cables are easily damaged when exposed to temperature and electromagnetic cycling, simulating ITER operational regimes, and that this microscale damage has a detrimental effect on superconducting properties. The root cause of the microscale damage is associated with electromagnetic (Lorentz) forces as well as thermally generated stresses due to cooling to cryogenic temperatures and residual stresses generated during the production process.25–28 Therefore, it is essential to assess and, if possible, to control the stress and strain state of the filaments, both when it originates from the manufacturing process and when it occurs due to the operating conditions. This knowledge can be used to predict and, ideally, eliminate possible damage to the superconducting filaments. In this respect, the residual stress is not only a partial cause of the damage, but also a quantity that can be studied to assess the degree of microscale damage. In case of development of microscale damage, the residual stresses become relaxed to a certain degree, and this effect can be studied experimentally.
Knowledge of the residual stresses is also important for understanding the effects of applied stress/strain on the superconducting properties, i.e. the critical current (Ic), which have been experimentally observed multiple times in MgB2 superconducting systems.29–32 The residual stresses were measured successfully on several occasions for Nb3Sn using neutron diffraction,33,34 and this technique proved to be the most suitable for the powder-in-tube system due to its ability to penetrate through the sheath material. There are no published results on measurements of the residual stress in MgB2 wires, however, presumably due to the fact that manufacturing 11B isotope based Mg11B2 wires is a prerequisite for such neutron measurements. Nevertheless, it is conceptually clear that, depending on the sign and magnitude of the residual stress, the combined effect of the residual and applied stress/strain can be different.
From this point of view, understanding the stress/strain behaviour of the Mg11B2 wires and coils for the magnet system of a fusion reactor is a critical issue in terms of current-carrying capability. Direct stress/strain measurements on the Mg11B2 filaments in the wire are difficult, because the Mg11B2 filamentary region, for practical use, is covered with a Monel (Ni–Cu alloy) sheath and Nb barrier. A high penetration depth of radiation, such as in the form of neutrons or high-energy synchrotron X-rays, is required to measure residual stress and texture on the superconducting wire.35
In this report, we used neutron diffraction for a full quantitative residual stress analysis of the constituents in 11B isotope based Mg11B2 wires (Mg11B2), in correlation with the fabrication conditions and the transport critical current density (Jc), for the first time. This assessment is the first step on the way to optimising the properties and manufacturing conditions for Mg11B2 superconductor intended for magnets in fusion reactors, with the possibility of mitigating unwanted stress and strain inside the wire filaments.
For neutron experiments, the individual Mg11B2 wires were cut into pieces ∼5 mm in length and bunched together to form bulk samples with approximate dimensions of 5 × 5 × 5 mm3. Measurements of residual stress were performed on the niobium, Mg11B2, and Monel phases. The measurements of residual stress on the Mg11B2 wires were carried out using the KOWARI neutron diffractometer42 at the Open Pool Australian Lightwater (OPAL) research reactor at the Australian Nuclear Science and Technology Organization (ANSTO). The Mg11B2 phase was measured in a 90° geometry using the wavelength λ = 1.5 Å for the Mg11B2 (211) reflection and gauge volume size of 4 × 4 × 4 mm3. Two principal directions, transverse and axial, were measured with constant rotation of the samples around their axis for better averaging.
A specially prepared pure Mg11B2 cylindrical pellet sample (5 mm diameter, 3 mm height) was used to determine the unstressed lattice spacing, d0. For the production of this pellet, a high temperature (HT) 800 °C thermal regime was used to produce a uniform (no Monel sheath, no Nb barrier) and high purity sample to ensure the absence of macro- and microstresses.
The stress (σ) was calculated for the measured transverse and axial strains, εt = (dt − d0)/d0 and εa = (da − d0)/d0, respectively, of the Mg11B2 (211) reflections in the corresponding directions using the (hkl)-dependent Young's modulus (E) and Poisson's ratio (ν) calculated from the single crystal elastic constants in the isotropic approximation, E (211) = 316.2 GPa, and ν (211) = 0.17. The two principal stress components, transverse and axial, were computed accordingly to the following relationship adapted for the case of the cylindrical symmetry stress state from the general Hooke's law.43,44 The cylindrical symmetry of the stress state reflects and inherits the cylindrical symmetry of the wire drawing process with only two distinct directions, axial and transverse.
To further study aspects of the anisotropic stress state, neutron texture measurements were performed on the wires, including three phases, Mg11B2, Monel sheath, and Nb barrier (only for the sample sintered at 700 °C, since the other samples were essentially identical). Several representative pole figures were collected to judge the crystallographic isotropy/anisotropy using the same KOWARI diffractometer. We consider that the effect of crystallographic texture,45 which requires experimental determination, is three fold. First, it determines the anisotropy of the elastic and thermal properties (e.g. Young's modulus and the coefficient of thermal expansion), which is important for proper stress calculation procedures, as well as for stress evaluation if a finite element method (FEM) simulation is to be done. Second, if some crystallographic preferred orientation is found, it can shed light on the mechanism of MgB2 phase formation and growth in the sintering process. Third, for the polycrystalline layered superconductors, e.g. yttrium barium copper oxide (YBCO), with extremely high anisotropy of the critical current, the effect of texture is so high that the current can be practically destroyed due to unfavourable crystallographic alignment of the grains.46 Although the single crystal anisotropy of MgB2 is much less pronounced, control of the degree of preferred orientation is required.
Fig. 2(a) shows that the cross-sectional microstructure of the wire consists of 49 vol% Monel, 28 vol% Nb, and 23 vol% Mg11B2. Fig. 2(b) presents the XRD patterns of the superconducting ceramic from the core of the Mg11B2 wires after sintering for one hour at 700 °C, 750 °C, and 800 °C. While the major peaks are indexed as Mg11B2 phase, unreacted Mg, MgO, and 11B-rich phase47,48 are present in the samples. Fig. 2(c) shows the volume fractions of the secondary phases as functions of the sintering temperature. In the wires sintered at 700 °C and 750 °C, there are certain amounts of retained 11B-rich phase and Mg phase, 10–20 vol%, sufficient to produce significant and measurable microstresses. Further increasing the heat-treatment to 800 °C diminished the volume fraction of the Mg and the 11B rich phase to 0.37% and 0.47%, respectively, resulting in the most fully reacted, most pure Mg11B2 superconductor.
Fig. 3 shows the experimental results for the residual stress measurements of Mg11B2 wires in the transverse and the axial directions, with error bars showing the estimated uncertainty due to neutron counting statistics. The wires were characterised to have tensile stress of 66 ± 15 MPa (HT 700 °C), 50 ± 15 MPa (HT 750 °C), and 6 ± 15 MPa (HT 800 °C) for the transverse component, which had a tendency to decrease with increasing heat-treatment temperature to almost negligible in the HT 800 °C sample.
The approach of the stress analysis and interpretation is based on the decomposition of the total stress into micro- and macro-stress.49 In the given system it is deemed that both components are present due to the structure of the wire, there is an inner core, which is by itself is a composite material, and there is also a possible interaction between that core and our metal sheath.
The main contribution to the total stress was hydrostatic microstress (phase incompatibility stress) due to the interaction between the Mg11B2 matrix and the elastically harder 11B rich phase upon cooling down from the sintering temperature.50 It is generated due to the difference in the thermal expansion of the phases. This microstress is assumed fully thermally generated, since MgB2 phase is synthesised during the heat-treatment process, and isotropic, since all constituent phases are crystallographically isotropic. This experimental result was corroborated by evaluating thermally generated phase stresses using a micromechanical model of the isotropic particulate composite based on the Eshelby inclusion formalism.51,52 The calculations were made accordingly to the evaluated volume fractions (Fig. 2) of the constituents (Mg11B2 as the primary phase, plus unreacted 11B rich phase inclusions) and the thermal conditions for the composite formation in the Mg–B phase diagram.53 A good numerical agreement with the experimental results was achieved. (Fig. 3 combines the experimental and calculated results.) Thus, based on the XRD phase analysis results and the residual stress neutron measurements, it can be concluded that the higher heat-treatment temperature of 800 °C is required for the full reaction of the 11B rich and Mg phases to form Mg11B2, which ensures a low level of residual microstress.
In the axial direction, some compressive contribution to the total stress is present in addition to the hydrostatically-compressive microstress contribution discussed above, thus bringing the stress in the axial direction from tensile to less tensile, or even into compressive range, as in the 800 °C heat-treated wire. This effect can be explained by the interaction between the Monel-Nb sheath and the Mg11B2, and is due to thermally generated macrostress. Taking account of the differences in the coefficient of thermal expansion (CTE) of the sheath and wire interior (Δα) and the temperature drop from the sintering temperature to room temperature (ΔT), the thermal strain mismatch Δε = ΔT·Δα determines the sign and magnitude of the macrostress in the sheath and in the interior of the wire. Based on the CTEs of the constituents, α (Mg11B2) = 8.3 × 10−6/K,54 α (Monel) = 14 × 10−6/K,55 and α (Nb) = 7.3 × 10−6/K,56 a compressive axial stress should be generated in Mg11B2, compensated by the tensile stress in the Monel sheath. In the wires sintered at 700 °C and 750 °C, with some amount of unreacted Mg phase and 11B rich phase, the same consideration is supposed to include Mg (α = 24.8 × 10−6/K)57 and 11B (α = 6 × 10−6/K)58 as well as microstructure features (e.g. possible pores and cracking). The resultant effect is highly sensitive to the conditions on the contact between the Monel tube and the Mg11B2 composite interior. Yet another explanation of this partial stress relaxation in the axial direction could be the presence of oriented cracks and pores arising from contraction during the sintering process and the pores originating from the Mg11B2 phase formation reaction in the heat-treatment procedure.
Fig. 4(a–d) shows the microstructure in the longitudinal direction of the Mg11B2 wires sintered at 700 °C, 750 °C, and 800 °C. These secondary electron image (SEI) observations indicate that aggregation occurs along with the presence of some small pores and microcracks in the 700 °C and 750 °C wires (Fig. 4(a and b)), while cracking and pores are more pronounced in the wire heat-treated at 800 °C (Fig. 4(c and d)). As the heat-treatment temperature increases, the aggregation of the Mg11B2 growth proceeds continuously while creating pores. As a result of the aggregation, Mg11B2 has a porous structure, and it can be easily damaged by thermal stress caused by the temperature drop from above 700 °C to room temperature.
Fig. 4 Low-vacuum SEM images of longitudinal sections of Mg11B2 wires heat-treated at (a) 700 °C, (b) 750 °C, and (c and d) 800 °C. |
Although the pores provide a precondition for the cracking-susceptible microstructure, the actual origin and mechanism of stress generation is twofold. First, due to the difference in CTE between the Monel/Nb sheath and the superconducting material, macrostress is generated, which in circumstances of porous microstructure leads to stress concentration. Second, due to the anisotropic thermal expansion of Mg11B2 (hexagonal crystal structure, α(a) = 5.4 × 10−6/K, α(c) = 11.4 × 10−6/K (ref. 59)), when the grains are randomly oriented, microstresses can also be generated. Although the overall average volume of these stresses is zero, the localised stresses can reach very large values, up to ∼1 GPa accordingly to our estimates. Thus, through these thermal mechanisms, very high magnitude and locally concentrated stress fields are generated, leading to microcrack formation conditions. The exact morphology, phase composition, and other details of the microstructure play roles in the actual stress state of the superconducting material. Thus, the more porous structure of the 800 °C sample makes it more cracking-prone than the lower temperature samples (700 °C and 750 °C) with more homogeneous structures. Also, while in less pure samples (700 °C and 750 °C), the local stress/strain fields can be accommodated by the plastically soft metallic Mg phase, this mechanism is substantially suppressed in the most pure (800 °C) sample, and thus, cracks are more easily formed in the 800 °C sample. Therefore, due to these two mechanisms, the most significant cracks on the scale of several microns are formed in the 800 °C sample.
Furthermore, the brittle fracturing leads to extensive cracking in the Mg11B2 structure, as seen in Fig. 4(c and d), resulting in a harmful effect on the transport Jc properties in Mg11B2 wire.60,61 In fact, it was previously reported in our research results that the wire sintered at 800 °C did not show a transport Jc, even though the sample was fully reacted with a high Mg11B2 superconducting phase fraction.62 On the other hand, the wire sintered at 750 °C has a superior transport critical current density, Jc = 2 × 104 A cm−2 at 4.2 K and 5 T compared with the multifilament wire manufactured by the National Institute for Fusion Science (NIFS).62 Therefore, based on the above discussion, the cracks and the pores have a detrimental influence on Jc through fracturing of the inter-grain connections, while, at the same time, these defects act as stress relief factors in the Mg11B2 wire sintered at 800 °C.
The superconducting transition temperature (Tc) was observed at a temperature of 36.5 K and 36.9 K, for the samples sintered at 700 °C and 800 °C, respectively.62 Compared to the reported results, e.g. 39.2 K in,63 the lower Tc in the present samples is most likely due to the presence and complex interactions of different types of MgB2 lattice defects, such as lattice strains/stresses, poor crystallinity, the presence of point defects and defects with higher dimensions, and issues with chemical purity and phase purity (e.g. the presence of small amounts of MgO).64 The exact role of each factor might be difficult to address, however due to the intertwined nature of these mechanisms.65