Bis-phenylethynyl polyhedral oligomeric silsesquioxanes: new high-temperature, processable thermosetting materials

Levi M. J. Moore*a, Jacob J. Zavalab, Jason T. Lambb, Josiah T. Reamsb, Gregory R. Yandeka, Andrew J. Guenthner*ac, Timothy S. Haddadb and Kamran B. Ghiassi*a
aAir Force Research Laboratory, Aerospace Systems Directorate, Edwards AFB, California 93524, USA. E-mail: levi.moore.1@us.af.mil; kamran.ghiassi@us.af.mil
bERC Incorporated, Edwards AFB, California 93524, USA
cNano Hydrophobics, Inc., San Francisco, CA 94115, USA. E-mail: andrewguenthner@gmail.com

Received 12th July 2018 , Accepted 20th July 2018

First published on 31st July 2018


Abstract

Bis-phenylethynyl polyhedral oligomeric silsesquioxane (bis-PE-POSS) compounds were synthesized and thermally cured yielding crosslinked materials. After curing at 370 °C, thermal decomposition occurs near 600 °C under nitrogen. These materials were synthesized by condensation of a new phenylethynyl-functional dichlorosilane onto tetrasilanol phenyl POSS, yielding two geometric isomers.


Various composite applications, especially in aerospace, call for polymeric matrix materials with high glass transition temperatures (Tgs) and good thermo-oxidative stability, able to withstand exposure to temperatures in excess of 300 °C while maintaining their mechanical robustness.1 A continuous service temperature of 370 °C is widely recognized as a very important technical challenge for organic matrix composites.2 Some thermosetting systems, such as polycyanurates,3,4 poly(benzoxazines),5 and phenylethynyl-endcapped poly(oligoimides)6 have approached that benchmark, but few resins possess the requisite combination of processability, mechanical properties, and thermo-oxidative stability. Those that can be utilized in service over 300 °C have finite lifetimes, especially in the presence of oxidizing species, and exhibit poor processability, requiring solvents for fiber impregnation and high pressures to promote flow. A matrix material that shows a significant improvement in thermochemical stability at high temperatures with an expanded processing window without the utilization of solvents would be a major step forward in the pursuit of next-generation resins.

One of the first examples of advancement towards this goal is NASA's PETI (phenylethynyl-terminated imide) series of phenylethynyl endcapped poly(oligoimide) resins.7–9 They exhibit high glass transition temperatures, excellent solvent resistance, and good mechanical properties, but have relatively poor flow characteristics, often requiring pressure during implementation of complex curing cycles. The robustness of the material can be attributed to the rigidity afforded by the many imide groups in the polymer, as well as phenylethynyl (PE) crosslinking chemistry, yielding a material with a broad processing window and good thermo-oxidative stability.

Common in high temperature thermosets, phenylethynyl crosslinking chemistry is a versatile route for the production of a variety of thermosetting materials. The robustness of this chemistry comes from the apparent cyclization of three phenylethynyl groups to form hexasubstituted benzene rings as the crosslink junctions in the final product, as well as higher order rings and other ill-defined but still olefinic structures.6,10 The properties of the final material are highly modular, with the crosslink density and molecular weight between crosslinks readily tunable through the size of the oligomer or polymer between the phenylethynyl groups.9

Also of note for their thermo-oxidative stability, polyhedral oligomeric silsesquioxane (POSS) compounds are hybrid organic–inorganic molecules composed of an inorganic silicon oxide core with an organic corona, well studied and available with a variety of functional groups. Phenyl-substituted POSS compounds are the most thermally stable in their class, due to their high aromatic content as well as the inorganic silsesquioxane core.11 Phenyl POSS compounds have found utility as additives for viscosity modification in high-temperature polymers, imparting improved processability and thermal properties when blended into the neat polymer, with little to no sacrifice in mechanical properties.12,13

There have been many efforts to covalently attach POSS to polymeric materials as well,14 including into polyimides as pendent moieties15,16 or even as monomers in the backbone of the polymer.17,18 This sort of incorporation increases the service lifetime of the fabricated part by reducing the amount of wear experienced. When exposed to low-Earth-orbit, Kapton-like polyimides with POSS moieties incorporated into the main chain of the polymer experienced erosion much more slowly than that of the neat polyimide due to the formation of a passivating silica layer.19 Additionally, phenylethynyl-functional POSS polyimide oligomers were found to be readily crosslinkable through the standard phenylethynyl cure schedule.20 These POSS-containing thermosets showed reduced moisture uptake when compared to the control polyimide, accomplished by the inclusion of the hydrophobic silsesquioxane cage of the POSS moieties, although with a reduction in the Tg of the finished material compared to the control. A strategy was developed to design a new matrix material that combined the high temperature properties of the POSS and phenylethynyl groups without any adverse effects of moisture uptake by removing the intermediate imide linkages. Here we present a new material, bis-PE-POSS, which utilizes the hybrid POSS architecture along with phenylethynyl curing chemistry. We report the synthetic route to this compound and demonstrate its exceptional thermal stability, with 5% mass loss temperatures approaching 600 °C.

POSS compounds are highly modular, and are commercially available with a variety of organic corona functionalities and reactive groups. This report builds on the library of functionalities available for condensation onto open POSS cages, yielding a compound with exceptional thermal stability. This synthetic procedure was modified from our previous report on the synthesis of aromatic POSS dianilines21,22 by the preparation of the phenylethynyl dichlorosilane (Scheme 1), yielding thermally robust compounds with a largely aromatic organic corona. Phenylethynyl bromide is reacted with magnesium turnings in THF to yield the Grignard reagent (1) as an emerald green solution which, after filtration to remove the unreacted magnesium, is added dropwise to excess methyltrichlorosilane in THF to yield the phenylethynyl methyl dichlorosilane (2). This dichlorosilane is a pale yellow solid and is easily purified through sublimation or recrystallization from hexanes, yielding pure product as seen by 29Si NMR (detailed synthetic procedures, NMR, and FTIR spectra are provided in the ESI).


image file: c8ra05954c-s1.tif
Scheme 1 Synthetic route to bis-PE POSS.

To condense the phenylethynyl dichlorosilane onto the POSS cage, the phenyl tetrasilanol POSS was first dissolved in THF, and a THF solution of triethylamine and dichlorosilane, both at a slight excess with respect to the silanol functionality, was added dropwise. Due to the asymmetry of the dichlorosilane, with a methyl group and a phenylethynyl group attached to the silicon, there are two different conformations that the resulting condensed cages can adopt, termed cis and trans. The cis isomer has both phenylethynyl groups arranged pointing the same way, and the trans has them both pointing opposite each other, leading to a more crystalline material that readily packs.

This subtle variation in crystal packing led to a difference in solubility between the two isomers. A solid precipitate formed in the reaction mixture after the condensation step that contained both triethylamine hydrochloride and the trans-bis-phenylethynyl POSS. After filtration of the reaction mixture, the filter cake was washed with methanol, and then stirred in methanol to remove any remaining salt, yielding pure trans-bis-phenylethynyl POSS. Less-crystalline cis-bis-phenylethynyl-POSS cages remained in solution, along with some trans-isomer. The filtrate was reduced in volume and precipitated into methanol. The solids were removed by filtration, which yielded a mixture of cis- and trans-isomers. Pure cis-isomer was obtained by selective extraction of the mixture with diethyl ether, in which the trans isomer is only sparingly soluble. Hansen solubility parameters were calculated based on group contribution models for POSS compounds,23 and despite the isomers' significant solubility differences, both compounds have estimated values of δD = 19.4 ± 0.6, δP = 6.9 ± 2.0, and δH = 5.7 ± 1.6. Estimated “radius of interaction” values (for minimal solubility) of the isomers, though, are around 12–16 for the cis compound compared to only 6–10 for the trans compound (see ESI). After isolation of the two different compounds, mixtures of cis- and trans-isomers were then formulated to determine the effect of stereochemistry on thermal properties.

The 29Si NMR spectra of the bis-phenylethynyl-POSS isomers are shown in Fig. 1. The full spectrum (a) shows a mixture of both isomers, as does (b), which along with the cis isomer in (c) and trans isomer in (d) are zoomed in to the regions of interest. Sharp peaks demonstrate that the POSS cages retain their discrete molecular structure through the functionalization step. The chemical shift from the silicon atoms that tether the phenylethynyl groups to the POSS cage is evident at −31.1 ppm (highlighted in blue), and the shifts from the two silicon atoms that are attached to the tethering silicon (through oxygens) are evident at −78.2 ppm (red). The central silicon atoms, then, show different shift patterns depending on the isomer. Because of the high symmetry of the trans isomer, the central silicon atoms exhibit only one peak (purple). The cis isomer's central silicon atoms are in differing chemical environments, with the shifts from the two atoms opposite the phenylethynyl groups at −79.6 ppm (green), and the shifts from the atoms between the phenylethynyl groups appearing at −79.1 ppm (orange).24


image file: c8ra05954c-f1.tif
Fig. 1 29Si NMR spectra of bis-PE POSS isomers. The full spectrum of a mixture of isomers is shown in (a), and zoomed in to the regions of interest in (b). The cis-isomer is shown in (c), and the trans-isomer in (d). Residual trans-isomer is evident in the spectrum for the cis-isomer (c).

Single crystals suitable for X-ray diffraction were grown from concentrated solutions of benzene containing either cis or trans bis-PE-POSS. The crystal structures, presented in Fig. 2, clearly show the different orientations between the regioisomers. While both structures are found in the same space group (triclinic, P[1 with combining macron]), the cis isomer is found on a crystallographic general position, while the trans isomer resides on a center of inversion. Interestingly, the structures suggest that the cis isomer belongs to the C2v point group while the trans is C2h.


image file: c8ra05954c-f2.tif
Fig. 2 X-ray crystal structures for cis (top) and trans (bottom) regioisomers of the bis-PE POSS compounds. Thermal ellipsoids are plotted at 30%. Colors represent silicon (blue), oxygen (red) and carbon (black). Hydrogen positions and solvate molecules are omitted for clarity.

Thermal studies were performed in order to ascertain the processability and thermal properties of the bis-PE-POSS compounds. Differential scanning calorimetry (DSC) showed distinct melting temperatures for the two isomers (Fig. 3a). Melting endotherms were observed for both isomers, with the cis-isomer showing a melting transition at 261 °C and the trans-isomer at 304 °C. The cis-isomer's lower crystallinity led to its lower melting point. The blend of the isomers exhibits two endotherms as expected. The cis-isomer showed no change in melting point in the mixture, but the trans-isomer saw a depression in melting point to 280 °C, presumably from solubilization into the cis-isomer. The compounds are free-flowing thin liquids in the melt state before cure. Both isomers and mixtures of isomers showed a cure exotherm with a maximum temperature around 379 °C. A representative exotherm is shown in Fig. 3b.


image file: c8ra05954c-f3.tif
Fig. 3 Differential scanning calorimetry curves (exo up) for cis, trans, and a 50[thin space (1/6-em)]:[thin space (1/6-em)]50 mixture of bis-PE-POSS showing melting points (a). Representative cure exotherm for a 50[thin space (1/6-em)]:[thin space (1/6-em)]50 mixture of bis-PE-POSS isomers (b).

Thermogravimetric analysis shows the exceptional thermal stability of these compounds. TGA curves are shown in Fig. 4, and detailed thermal properties are shown in Table 1. The phenylethynyl groups on the POSS cage crosslink and cure above 320 °C with a maximum rate at 370 °C, leading to a highly crosslinked system with increased aromatic character compared to the discrete molecules themselves. The cis isomer, trans isomer, or a 50/50 mixture of the two were cured in situ in a TGA pan with an isothermal hold at 370 °C for 1 h. The resulting cured bis-PE-POSS resin was then subjected to a ramp to 1000 °C at a rate of 10 °C min−1. In a nitrogen atmosphere, 5% mass loss occurred around 595 °C for each isomer, as well as the mixture of isomers. The char yields are also quite high, all around 77%. For comparison, a known phenylethynyl-endcapped polyimide, 6-FDA-ODA-PEPA,20 was subjected to the same thermal treatment, and shows a 5% mass loss temperature of 574 °C and a char yield of 57%. Analysis in air shows quite high degradation temperatures as well. The polyimide left no char yield after ramping to 1000 °C, but the char yields of the bis-PE POSS compounds in air were 43% for the trans isomer, 36% for the cis isomer, and 39% for the mixture, all close to the theoretical value for the mass fraction of the central inorganic cage. The carbonaceous content of the cured resin was oxidized and lost, leaving behind the nonvolatile silicon oxide portions of the resin.


image file: c8ra05954c-f4.tif
Fig. 4 TGA curves of bis-PE-POSS in nitrogen (solid lines) and air (dashed lines).
Table 1 Thermal properties of in situ cured bis-PE-POSS resin
Material Atmosphere 5% loss T (°C) Char yield (%)
trans-bis-PE-POSS N2 596 78
Air 559 43
cis-bis-PE-POSS N2 594 77
Air 548 36
50[thin space (1/6-em)]:[thin space (1/6-em)]50 trans[thin space (1/6-em)]:[thin space (1/6-em)]cis-bis-PE-POSS N2 592 76
Air 571 39
6-FDA-ODA-PEPA N2 574 57
Air 564 0


These compounds show an increase in degradation temperature as compared to other phenyl substituted POSS compounds as well. Octaphenyl POSS has a degradation and volatilization temperature around 450 °C and char yield of 70% in nitrogen,11,25 well below that of the bis-PE-POSS. The crosslinking and increase in aromatic content in the bis-PE POSS compounds improves thermal stability compared to other POSS systems, leading to a more robust material.

Conclusions

In conclusion, we have synthesized a phenylethynyl-functional POSS compound through a modular synthesis that shows exceptional thermal stability to temperatures approaching 600 °C. This compound is able to be utilized as a thermoset resin, and is crosslinked through cyclization of its phenylethynyl groups. This crosslinking process greatly enhances its thermal stability in comparison to high temperature polymers, and even improves on properties seen in POSS compounds with similar functionality through inclusion of the curable phenylethynyl group. This compound opens up the possibility of thermoset resins with ever greater thermal stabilities and operational temperatures.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by the Air Force Office of Scientific Research and by the Air Force Research Laboratory Rocket Propulsion Division. Work at the Molecular Foundry was supported by the Office of Science, Office of Basic Energy Sciences, of the U.S. Department of Energy under Contract No. DE-AC02-05CH11231.

Notes and references

  1. I. Hamerton and L. Mooring, The Use of Thermosets in Aerospace Applications, in Thermosets, ed. Q. Guo, Woodhead Publishing, 2012, pp. 189–227 Search PubMed.
  2. National Research Council, Structural and Multifunctional Materials, in Materials Research to Meet 21st-Century Defense Needs, The National Academies Press, Washington, DC, 2003, pp. 27–54 Search PubMed.
  3. I. Hamerton and J. N. Hay, Recent Developments in the Chemistry of Cyanate Esters, Polym. Int., 1998, 47, 465–473 CrossRef.
  4. A. J. Guenthner, V. Vij, T. S. Haddad, J. T. Reams, K. R. Lamison, C. M. Sahagun, S. M. Ramirez, G. R. Yandek, S. C. Suri and J. M. Mabry, Silicon-Containing Trifunctional and Tetrafunctional Cyanate Esters: Synthesis, Cure Kinetics, and Network Properties, J. Polym. Sci., Part A: Polym. Chem., 2014, 52, 767–779 CrossRef.
  5. S. Rimdusit, S. Tiptipakorn, J. Jubsilp and T. Takeichi, Polybenzoxazine alloys and blends: Some unique properties and applications, React. Funct. Polym., 2013, 73, 369–380 CrossRef.
  6. Y. Li and R. J. Morgan, Thermal Cure of Phenylethynyl-Terminated AFR-PEPA-4 Imide Oligomer and a Model Compound, J. Appl. Polym. Sci., 2006, 101, 4446–4453 CrossRef.
  7. R. G. Bryant, B. J. Jensen and P. M. Hergenrother, Chemistry and Properties of a Phenylethynyl-Terminated Polyimide, J. Appl. Polym. Sci., 1996, 59, 1249–1254 CrossRef.
  8. B. J. Jensen, R. G. Bryant, J. G. Smith Jr. and P. M. Hergenrother, Adhesive Properties of Cured Phenylethynyl-Terminated Imide Oligomers, J. Adhes., 1995, 54, 57–66 CrossRef.
  9. D. Lee, H. V. Tippur, B. J. Jensen and P. B. Bogert, Tensile and Fracture Characterization of PETI-5 and IM7/PETI-5 Graphite/Epoxy Composites Under Quasi-Static and Dynamic Loading Conditions, J. Eng. Mater. Technol., 2011, 133, 021015 CrossRef.
  10. X. Fang, X.-Q. Xie, C. D. Simone, M. P. Stevens and D. A. Scola, A Solid-State 13C NMR Study of the Cure of 13C-Labeled Phenylethynyl End-Capped Polyimides, Macromolecules, 2000, 33, 1671–1681 CrossRef.
  11. A. Fina, D. Tabuani, F. Carniato, A. Frache, E. Boccaleri and G. Camino, Polyhedral oligomeric silsesquioxanes (POSS) thermal degradation, Thermochim. Acta, 2006, 440, 36–42 CrossRef.
  12. K. M. Knauer, G. Brust, M. Carr, R. Cardona, J. D. Lichtenhan and S. E. Morgan, Rheological and crystallization enhancement in polyphenylenesulfide and polyetheretherketone POSS nanocomposites, J. Appl. Polym. Sci., 2017, 134, 44462 CrossRef.
  13. H. W. Milliman, M. Sanchez-Soto, A. Arostegui and D. A. Schiraldi, Structure–property evaluation of trisilanolphenyl POSS®/polysulfone composites as a guide to POSS melt blending, J. Appl. Polym. Sci., 2012, 125, 2914–2919 CrossRef.
  14. A. Kausar, State-of-the-Art Overview on Polymer/POSS Nanocomposite, Polym.-Plast. Technol. Eng., 2017, 56, 1401–1420 CrossRef.
  15. M. E. Wright, B. J. Petteys, A. J. Guenthner, S. Fallis, G. R. Yandek, S. J. Tomczak, T. K. Minton and A. Brunsvold, Chemical Modification of Fluorinated Polyimides: New Thermally Curing Hybrid Polymers with POSS, Macromolecules, 2006, 39, 4710–4718 CrossRef.
  16. C. Leu, Y. Chang and K. Wei, Synthesis and Dielectric Properties of Polyimide-Tethered Polyhedral Oligomeric Silsesquioxane (POSS) Nanocomposites via POSS-diamine, Macromolecules, 2003, 36, 9122–9127 CrossRef.
  17. S. Wu, T. Hayakawa, R. Kikuchi, S. J. Grunzinger and M. Kakimoto, Synthesis and Characterization of Semiaromatic Polyimides Containing POSS in Main Chain Derived from Double-Decker-Shaped Silsesquioxane, Macromolecules, 2007, 40, 5698–5705 CrossRef.
  18. A. L. Brunsvold, T. K. Minton, I. Gouzman, E. Grossman and R. Gonzalez, An Investigation of the Resistance of Polyhedral Oligomeric Silsesquioxane Polyimide to Atomic-Oxygen Attack, High Perform. Polym., 2004, 16, 303–318 CrossRef.
  19. T. K. Minton, M. E. Wright, S. A. Marquez, L. Shen, A. L. Brunsvold, R. Cooper, J. Zhang, V. Vij, A. J. Guenthner and B. J. Petteys, Atomic Oxygen Effects on POSS Polyimides in Low Earth Orbit, ACS Appl. Mater. Interfaces, 2012, 4, 492–502 CrossRef PubMed.
  20. D. M. Pinson, G. R. Yandek, T. S. Haddad, E. M. Horstman and J. M. Mabry, Thermosetting Poly(imide silsesquioxane)s Featuring Reduced Moisture Affinity and Improved Processability, Macromolecules, 2013, 46, 7363–7377 CrossRef.
  21. B. Seurer, A. Lee, V. Vij, T. Haddad and J. Mabry, Thermal Transitions and Reaction Kinetics Polyhedral Silsesquioxane-containing Phenethynylphthalimides, Macromolecules, 2010, 43, 9337–9347 CrossRef.
  22. V. Vij, T. S. Haddad, G. R. Yandek, S. M. Ramirez and J. M. Mabry, Synthesis of Aromatic Polyhedral Oligomeric Silsesquioxanes (POSS) Dianilines for Use in High-Temperature Polyimides, Silicon, 2012, 4, 267–280 CrossRef.
  23. A. J. Guenthner, K. R. Lamison, L. M. Lubin, T. S. Haddad and J. M. Mabry, Solubility Parameters for Octahedral Oligomeric Silsesquioxanes, Ind. Eng. Chem. Res., 2012, 51, 12282–12293 CrossRef.
  24. B. W. Schoen, D. Holmes and A. Lee, Identification and quantification of cis and trans isomers in aminophenyl double-decker silsesquioxanes using 1H-29Si gHMBC NMR, Magn. Reson. Chem., 2013, 51, 490–496 CrossRef PubMed.
  25. G. R. Yandek, B. M. Moore, S. M. Ramirez and J. M. Mabry, Effects of Peripheral Architecture on the Properties of Aryl Polyhedral Oligomeric Silsesquioxanes, J. Phys. Chem. C, 2012, 116, 16755–16765 CrossRef.

Footnote

Electronic supplementary information (ESI) available: Detailed synthetic procedures, NMR spectra of all new compounds, FTIR spectra, elemental analysis, single crystal X-ray crystallographic data, TGA details, and estimation of Hansen solubility parameters. CCDC 1839015 and 1839016. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/c8ra05954c

This journal is © The Royal Society of Chemistry 2018
Click here to see how this site uses Cookies. View our privacy policy here.