Electrospinning preparation of a large surface area, hierarchically porous, and interconnected carbon nanofibrous network using polysulfone as a sacrificial polymer for high performance supercapacitors

Wenyu Wang*a, Hongjie Wanga, He Wanga, Xin Jinb, Jialu Lia and Zhengtao Zhu*ac
aState Key Laboratory of Separation Membranes and Membrane Processes, School of Textiles, Tianjin Polytechnic University, Tianjin 300387, China. E-mail: wwy-126.com
bSchool of Materials Science and Engineering, Tianjin Polytechnic University, Tianjin 300387, China
cDepartment of Chemistry and Applied Biological Science, South Dakota School of Mines and Technology, Rapid City, SD 57701, USA. E-mail: zhengtao.zhu@sdsmt.edu

Received 12th July 2018 , Accepted 2nd August 2018

First published on 9th August 2018


Abstract

Carbon nanofibrous mats (CNFMs) are prepared by electrospinning of blended precursor of polyacrylonitrile and polysulfone (PSF) followed by pre-oxidation stabilization and carbonization. Addition of PSF as a sacrificial polymer leads to CNFMs with high surface area, large numbers of micropores and mesopores, good degree of carbonization, and interconnected fibrous network, due to the high decomposition temperature, release of SO2 during decomposition, and large amount of carbon residue of PSF during carbonization. The electrochemical characterization shows that the CNFM electrode has a specific capacitance of 272 F g−1 at a current density of 1 A g−1 with 74% of the specific capacitance retained at 50 A g−1 in 2.0 M KOH electrolyte. The CNFM electrodes have excellent cycling durability with 100% capacitance retention after 10[thin space (1/6-em)]000 cycles.


1. Introduction

Electrochemical energy storage systems are crucially important in the development of renewable, sustainable, and eco-friendly energy technologies because of the intermittent nature of the available renewable energy sources. Among various electrochemical energy storage devices, supercapacitors have attracted wide attention in recent years because of their fast charge–discharge rate, high power density, excellent cycle durability, and low fabrication/operation cost.1 In supercapacitors, particularly in the electrochemical double layer capacitors (EDLCs), the electrode materials largely determine the performance of the devices; therefore, considerable efforts have been devoted to develop advanced materials for supercapacitor electrode.2–5 Carbon nanofibrous mats (CNFMs) prepared from electrospinning have shown great potential as electrode materials for supercapacitors.6–9 For high performance supercapacitors, the ideal CNFMs need to have (1) large surface areas, (2) hierarchical pore structures, and (3) high electrical conductivity. In a supercapacitor, the electric charges are adsorbed and stored on the surface of the electrode, therefore, porous structures with large surface areas are required to have high charge storage capacity. Additionally, high surface areas may not necessarily result in high performance, since not all pores can be utilized for charge storage; hierarchical pore structures ranging from micropore (0.5–2 nm), mesopore (2–50 nm), and macropore (>50 nm) are desired for effective electrolyte ion transport and charge storage. Furthermore, high electric conductivity of CNFMs reduces the internal resistance of the supercapacitors.

CNFMs prepared by electrospinning and carbonization typically have limited surface area and conductivity. Many works have focused on preparation of CNFMs with high surface areas and desired porous structures. One approach is to use blended polymer precursor consisting of a carbon source polymer and a sacrificial polymer as spin dope to increase the surface areas and to control the pore sizes.10–14 The common sacrificial polymer (e.g., polymethylmethacrylate and polyvinylpyrrolidone) degrades completely without carbon residues at temperatures well below carbonization temperature, leading to porous structures of CNFMs. In general, the nanofibers produced by this method need to be further activated to increase the surface areas; and the pores produced are largely mesopores, which may not all contribute to the charge storage. The conductivity of CNFMs may be improved by increasing the carbonization temperature, which increases the graphitic carbon contents of individual nanofiber. To further improve the conductivity of CNFMs, interconnected fibrous networks of CNFMs are desired. Few studies have been reported to prepare the interconnected CNFMs, particularly the ideal electrode material of the interconnected CNFMs with high surface areas and hierarchical porous structures.15–17

Recently, we reported preparation of carbon nanofibrous mat by carbonization of electrospun nanofibers of polyacrylonitrile (PAN) and polysulfone (PSF) blends.18 As an in situ activation agent, PSF helped formation of CNFMs with increased mesopore content, specific surface area, graphitization degree, and conductivity of CNFMs. Slurries of CNFMs, carbon black, and poly(tetrafluoroethylene) were made into electrodes for two-electrode symmetric supercapacitor. The supercapacitor showed good performance, cycling stability, and energy capacity.

Herein, we report our further studies on the electrospun CNFMs prepared from the blended polymer precursor composed of PAN and PSF. Based on the morphological and structural characterization, thermal analysis, surface area and porosity measurements, we propose a detailed mechanism for formation of high surface area, microporous and mesoporous structure, well interconnected carbon nanofibrous network with good graphitic carbon contents of the PAN/PSF-based CNFMs. Furthermore, the electrochemical performance of the supercapacitor electrode prepared by the freestanding CNFMs without further activation and additives is characterized under high charge/discharge rate. The result shows a high specific capacitance of ∼272 F g−1 at 1 A g−1 current density and ∼200 F g−1 at a fast charge rate of 50 A g−1, demonstrating excellent electrochemical properties under fast charge/discharge conditions. The electrodes retain excellent cycling durability with 100% capacitance retention at 1 A g−1 rate after 10[thin space (1/6-em)]000 cycles.

2. Experimental

2.1. Materials

Polyacrylonitrile (PAN, Mw = 90[thin space (1/6-em)]000) was purchased from Spectrum Co., Ltd, Shanghai. Polysulfone (PSF, Mw = 55[thin space (1/6-em)]000) was obtained from Solvay Chemical Co., Ltd. N,N-Dimethylformamide (DMF) was purchased from Kemiou Chemical Reagent Co., Ltd, Tianjin. Potassium hydroxide (KOH, purity ≥ 85%) was obtained from Fengchuan Chemical Reagent Science and Technology Co., Ltd, Tianjin. Deionized water was used in all experimental processes.

2.2. Preparation of CNFMs

PSF and PAN were dissolved simultaneously in DMF to form a homogeneous precursor solution. The concentration of PAN and PSF was 8.0 wt% and 2.0 wt%, respectively, thus there was 20 wt% of PSF in the obtained PSF/PAN precursor nanofibers. For the electrospinning process, the spin dope was loaded in a syringe spinneret, and an applied voltage between the stainless-steel needle of the syringe and the grounded collector was set at 20 kV; the distance between the spinneret and the collector was 18 cm and the flow rate was set at 16.67 μL min−1. The as-spun PSF/PAN nanofibrous mat (denoted as NFM-20) was pre-oxidized at 280 °C in air for 1 hour after ramping the temperature to 280 °C at a rate of 2 °C min−1; then the pre-oxidized NFM-20 was carbonized at 800 °C in nitrogen for 2 hours after the temperature was ramped to 800 °C at a rate of 5 °C min−1. The obtained carbon nanofibrous mat from NFM-20 was denoted as CNFM-20. The electrospun PAN nanofibrous mat (denoted as NFM-0) without PSF and the subsequent carbon nanofibrous mat (CNFM-0) were prepared following the same procedure.

2.3. Characterization

The surface morphology of the nanofibers was observed using scanning electronic microscope (SEM, Gemini SEM500) and high-resolution transmission electron microscopy (HRTEM, JEM-2100F). The degree of carbonization was evaluated by X-ray diffraction spectrometer (XRD, D8 DISCOVER). Raman spectra were collected by a Raman spectrometer (Raman, XploRA PLUS) with a 532 nm excitation laser. The thermogravimetric data was acquired using STA449F3 analyzer at a scanning rate of 10 °C min−1 under nitrogen atmosphere. Thermal behaviors of the samples were characterized by differential scanning calorimeter (DSC, DSC 200F3) at a heating rate of 10 °C min−1 under nitrogen atmosphere. The surface chemical composition was analyzed by X-ray photoelectron spectroscopy (XPS, K-alpha) equipped with a 165 mm hemispherical electron energy analyzer. BET surface areas of the samples were determined using the nitrogen adsorption method on Autosorb-iQ-C. The electrical conductivity of the CNFs was measured using a semiconductor powder resistivity tester (ST-2722).

2.4. Fabrication and electrochemical characterization of CNFMs based supercapacitor

The freestanding CNFM was pressed directly on a circular nickel foam (diameter: 1.2 cm; loading: ∼2 mg) to be used as an electrode. For the three-electrode electrochemical measurement, Pt foil was used as the counter electrode, and Hg/HgO was used as the reference electrode. The 2.0 M KOH aqueous solution was employed as the electrolyte. The cyclic voltammetry (CV) was measured between 0 and −1.0 V at a scan rate of 10 mV s−1, and the galvanostatic charge/discharge (GCD) curves were collected at various current densities ranging from 1.0 A g−1 to 50 A g−1 by an electrochemical workstation (Zahner, Zennium 2.0+CIMPS-2). The retention rate of electrodes was evaluated at a current density of 1.0 A g−1 for 10[thin space (1/6-em)]000 cycles using a supercapacitor test system (LANHE, CT2001A). The electrochemical impedance spectroscopy (EIS) of the electrodes was measured at the open circuit voltage with an AC amplitude of 5 mV over the frequency range of 10 mHz to 10 kHz.

Two-electrode supercapacitor was fabricated using two identical CNFM electrodes with a piece of PP/PE composite as separator and 2.0 M KOH aqueous solution as electrolyte. The cyclic voltammetry (CV) was measured between 0 and 1.0 V at various scan rate, and the galvanostatic charge/discharge (GCD) curves were collected at various current densities ranging from 0.25 A g−1 to 50 A g−1 by an electrochemical workstation (Zahner, Zennium 2.0+CIMPS-2).

3. Results and discussion

SEM images of the as-prepared precursor nanofibrous mats, NFM-0 and NFM-20, are shown in Fig. S1. Both NFM-0 and NFM-20 have similar morphology with smooth and randomly overlaid nanofibers. For individual nanofiber, the diameter of the nanofiber is uniform. No beads are observed in the SEM images of both samples. SEM images of CNFM-0 with different magnifications are shown in Fig. 1a, a′ and a′′. Compared to the precursor PAN nanofibrous mat (i.e. NFM-0), the nanofibers of CNFM-0 are slightly curly, likely due to the shrinkage during carbonization. The average diameter of CNFM-0 is 190 ± 60 nm, smaller than that of NFM-0. The morphology of CNFM-20, which is carbonized from the PSF/PAN precursor fibrous mat (i.e. NFM-20), is shown in Fig. 1b, b′ and b′′. The diameter of CNFM-20 is 115 ± 65 nm, much smaller than that of CNFM-0. Compared with the nanofibers of CNFM-0, the individual nanofiber of CNFM-20 has more curly structure and nonuniform diameter. More importantly, the nanofibers of CNFM-20 are weld together at the fiber junction points to form an interconnected fibrous network (Fig. 1b′), whereas no welding to fuse the nanofibers at the fiber junction points for the PAN-derived CNFM-0 (Fig. 1a′). Fig. 1a′′ and b′′ show the high magnification cross-sectional SEM images of the nanofibers in CNFM-0 and CNFM-20, respectively; porous structures are observed ubiquitously throughout the nanofibers of the CNFM-20. The HRTEM image of the CNFM-20 in Fig. S2 shows that the CNFM-20 nanofibers have good microporous structures.
image file: c8ra05957h-f1.tif
Fig. 1 SEM images of CNFM-0 (a, a′ and a′′) and CNFM-20 (b, b′ and b′′).

The pore information of CNFM-0 and CNFM-20 including the BET specific surface area, microporous and mesoporous volumes is summarized in Table 1. The PAN based CNFM-0 has specific surface area of 96 m2 g−1; and the CNFM-20 from PSF/PAN has specific surface area of 763 m2 g−1, about 8 times higher than that of CNFM-0. As shown in Fig. 2a, CNFM-20 have higher nitrogen adsorbed volume at low pressure, indicating that the PSF/PAN based CNFM-20 has a better interfacial adsorption capacity than the PAN based CNFM-0. The surface area of the micropore in CNFM-20, measured by Langmuir method, is about 5 times higher than that of CNFM-0. The mesopore volume distribution of CNFM-20 and CNFM-0 is showed in Fig. S3, and the result clearly indicates that CNFM-20 has higher mesopore volume than CNFM-0. Overall, addition of PSF results in much higher surface areas and better hierarchical pore structures in CNFM-20. Fig. 2b shows the XRD patterns of CNFM-0 and CNFM-20. Both CNFMs have a strong diffraction peak at 2θ = 22° and a weak diffraction peak at 2θ = 16°, corresponding to the graphitic crystallite plane (002) and the PAN crystallite plane (100), respectively.19,20 Presence of the (100) peak indicates incomplete carbonization, which is likely due to the relative low carbonization temperature of 800 °C.21 With addition of PSF, the (100) peak becomes weaker and the (002) peak becomes stronger, indicating increase of the amount of the graphitic carbon in CNFM-20. Fig. 2c shows the Raman spectra of CNFM-0 and CNFM-20. The spectra of both samples show the typical G band (1585 cm−1) and D band (1350 cm−1) for carbonaceous materials. The G band is related to the ordered graphitic carbon, whereas the D band is related to the amorphous and disordered carbon. The spectrum of CNFM-20 shows a much stronger G band compared to the spectrum of CNFM-0, indicating higher content of the sp2 hybridized graphitic carbon in CNFM-20. The degree of carbonization is also evaluated by the intensity ratio (R) of the D and G bands (i.e. R = ID/IG).22 The R values of the CNFM-0 and CNFM-20 are 1.51 and 1.04, respectively. The low R value of the CNFM-20 confirms that addition of PSF improves the degree of carbonization in CNFM-20. The improved degree of carbonization and the interconnected nanofibrous morphology (Fig. 1b′) results in high conductivity of CNFM-20, as shown in Table 1. Fig. S4 shows the XPS characterization of the surface chemical compositions of the CNFMs. The surfaces of both CNFM-0 and CNFM-20 contain three elements, C, N, and O. The PSF/PAN based CNFM-20 has relatively high C contents compared to the PAN based CNFM-0. The percentage of each element is shown in the inset of Fig. S4. CNFM-20 has the higher carbon percentage (94.7%) than CNFM-0 (91.5%).

Table 1 Surface areas, pore parameters, conductivity, and capacitance of CNFM-0 and CNFM-20
CNFM Surface area and pore parameter Conductivity (S cm−1) Capacitance
SBETa (m2 g−1) Vtotb (cm3 g−1) Vmesoc (cm3 g−1) Vmicrod (cm3 g−1) Smicroe (m2 g−1) GCDf (F g−1)
a SBET: specific surface area by BET.b Vtot: total pore volume, measured at P/P0 = 0.995.c Vmeso: mesopore volume by BJH.d Vmicro: micropore volume by Langmuir.e Smicro: specific surface area by Langmuir.f Measured by galvanostatic charge/discharge (GCD) at 1.0 A g−1.
CNFM-0 96 0.14 0.13 0.01 225 6.64 138
CNFM-20 763 0.51 0.22 0.29 1035 13.85 272



image file: c8ra05957h-f2.tif
Fig. 2 (a) N2 adsorption/desorption isotherms of CNFM-0 and CNFM-20. (b) XRD patterns of CNFM-0 and CNFM-20. The graphitic crystallite plane (002) and the PAN crystallite plane (100) are labelled. (c) Raman spectra of CNFM-0 and CNFM-20. (d) TGA curves of PAN nanofibers, PSF/PAN nanofibers, and PSF.

The thermal behaviors of the CNFMs are investigated by TGA and DSC analysis. Fig. 2d shows the TGA curves of PSF, the PAN nanofibrous mat, and the PSF/PAN nanofibrous mat. The pristine PSF is stable with no weight loss below about 500 °C. It degrades quickly when the temperature exceeds 500 °C and loses about 60% of the weight from 500 to 600 °C; above 600 °C, the remaining PSF only loses small percentage of its weight, leaving about 32% of carbon residue. The result suggests that PSF decomposes completely between 500 to 600 °C and it is carbonized at relatively low temperature. The PAN nanofibrous mat starts to lose weight significantly above the pre-oxidation temperature of 280 °C; the weight loss slows down above ∼500 °C but continues during the carbonization process. The weight loss of the PSF/PAN nanofibrous mat is less than that of the PAN nanofibrous mat below ∼500 °C; above 500 °C, because of the quick decomposition of PSF, the PSF/PAN nanofibrous mat loses weight quickly. Eventually, the PSF/PAN nanofibrous mat has a slightly lower carbon yield in comparison with the PAN mat. Fig. S5 shows the result of DSC analysis of the pre-oxidation and carbonization process for preparation of both CNFM-0 and CNFM-20. The DSC curve of PAN nanofibrous mat has a pronounced exothermic peak at about 285 °C (due to pre-oxidation) and two broad exothermic peaks during carbonization.23 The DSC curve of the PSF polymer shows a glass transition temperature of ∼200 °C and a more pronounced endothermic transition at ∼500 °C, in consistence with decomposition of PSF observed in TGA measurement (Fig. 2d). It is worth noting that PSF typically has a melt processing temperature of ∼350 °C.24 Therefore, PSF may be in a low-viscosity melting state in the pre-oxidized CNFM-20 before decomposition at above 500 °C. As a result, the melted PSF polymer facilitates the formation of fibrous network of CNFM-20.

The interconnected fibrous network (Fig. 1b′) and the high content of graphitic carbon (as suggested by Fig. 2b and c) of CNFM-20 lead to high conductivity of the material. As shown in Table 1, the conductivity of PAN-derived CNFM-0 is 6.64 S cm−1; and the conductivity of PSF/PAN-derived CNFM-20 is 13.86 S cm−1, about twice that of CNFM-0.

Based on the XRD, Raman, XPS, and thermal analysis results, the high surface areas, hierarchical porous structures, good electric conductivity of CNFM-20 can be explained by the chemical and structural changes during pre-oxidation and carbonization process, as shown in Fig. 3. For CNFM-0 derived from the PAN nanofibers, it is well known that the stable cyclic ladder molecule structure and the six membered ring graphite structure are obtained during pre-oxidation and carbonization steps, respectively.25 As shown in Fig. 3a, no interconnection at the fiber junction points is formed, presumably because the stable cyclic ladder molecule structure during the pre-oxidation prevents melting/softening of PAN nanofibers to form connected junctions. In addition, the CNFM prepared from pure PAN nanofibers typically have smooth surface, resulting in small number of mesopores and micropores and low specific surface area. The formation of CNFM-20 from the PSF/PAN nanofibers is schematically shown in Fig. 3b. During the pre-oxidation process, similar formation of stable cyclic ladder molecule structure of PAN is expected with no chemical change of PSF because of the thermal stability of PSF at 280 °C. The PSF component in PSF/PAN becomes soft above the glass transition temperature (∼200 °C) and is further softened/melt at higher temperature before decomposition. After decomposition, the PSF molecular chains continue being carbonized with increase of the temperature. Since the PSF polymer chains are broken into short chains, these shortened chains would further act as a glue at fiber junction points to fuse the carbonized PSF/PAN nanofibers together during decomposition and carbonization. Moreover, the decomposition of PSF in the carbon nanofibers leads to formation of mesopores, which is an important factor for increase of the specific surface area in CNFM-20. As shown in Fig. 3c, the repeating unit of PSF contains four benzene rings and a sulfonate group, thus PSF has a high thermal degradation temperature of approximately 550 °C; furthermore, the sulfone group of the PSF molecule is released as the SO2 gas from the nanofibers.26–28 The release of SO2 contributes to the formation of micropores, increasing the Langmuir surface area in the PSF/PAN derived CNFM-20 (as shown in Table 1).


image file: c8ra05957h-f3.tif
Fig. 3 (a) Schematic illustration of formation of the PAN based CNFM-0. (b) Schematic illustration of formation of the PSF/PAN based CNFM-20. (c) The chemical structure of the repeating unit of PSF and the chemical change during decomposition.

The electrochemical performance of the CNFMs is investigated in a three-electrode configuration. The inset of Fig. 4a shows the images of CNFM-20 pressed directly on the nickel foam electrode. Fig. 4a shows the CV curves of both CNFM-0 and CNFM-20 at a scan rate of 10 mV s−1. Both CNFM-based electrodes have a near-rectangular shape, indicating excellent EDLC behavior and low internal resistance. The slight increase of current below −0.8 V may be due to the pseudocapacitive contribution from the N and/or O groups in CNFMs (Fig. S4), which is common in the porous carbon electrode materials.29 The CV curve of CNFM-20 has larger rectangular area compared to that of CNFM-0, indicating higher capacitance of CNFM-20.


image file: c8ra05957h-f4.tif
Fig. 4 (a) CV curves of CNFM-0 and CNFM-20. Inset: the images of the nickel foam (left) and the CNFM-20 nanofibrous mat pressed on the nickel foam (right). (b) GCD curves of CNFM-0 and CNFM-20 at current density of 1.0 A g−1. (c) Cyclic performance of CNFM-0 and CNFM-20 measured at current density of 1.0 A g−1. Inset: specific capacitances of CNFM-0 and CNFM-20 at current densities from 1.0 A g−1 to 50 A g−1. (d) Nyquist plots of the impedance of CNFM-0 and CNFM-20.

Fig. 4b shows the GCD behavior of the CNFMs at a current density of 1.0 A g−1 in a three-electrode configuration and 2.0 M KOH electrolyte. The GCD curves of the CNFMs at different current densities are shown in Fig. S6. The triangular shape of the GCD curves at various current densities indicates efficient ionic and electronic transport and good EDLC formation in both CNFM electrodes. CNFM-20 prepared from the PSF/PAN nanofibers have longer discharge time than the PAN based CNFM-0; the result is consistent with the higher capacitance in CNFM-20 observed in the CV measurement. The specific capacitance of the electrode (listed in Table 1) is calculated using the following eqn (1) from the GCD curve.30

 
image file: c8ra05957h-t1.tif(1)
where Cs (F g−1) is the specific capacitance, ΔV (V) is the potential change within the discharge time Δt (s), m (g) is the mass of the active materials, and I (A) is the set current of the GCD measurement. The CNFM-20 electrode has a specific capacitance of 272 F g−1, while the CNFM-0 electrode shows a specific capacitance of 138 F g−1. The GCD specific capacitances of both CNFMs at charging rate from 1 A g−1 to 50 A g−1 are shown in the inset of Fig. 4c. At a high current density of 50 A g−1, the CNFM-20 and CNFM-0 electrodes retain 74% and 44% of the specific capacitances at the current density of 1.0 A g−1, respectively. The coulombic efficiency, defined as the ratio of discharge time and charge time at the same current density, for the electrode of CNFM-20 is 80%, whereas the coulombic efficiency for the electrode of CNFM-0 is 73%. The high retention rate and coulombic efficiency of the CNFM-20 electrode indicates the excellent supercapacitor performance of the materials, which originates from the high surface areas, hierarchical porous structure and interconnected carbon nanofiber network of CNFM-20. To further evaluate the cycle performance, the CNFM electrodes in three-electrode configuration are charged and discharged repeatedly for 10[thin space (1/6-em)]000 cycles at a current density of 1.0 A g−1 in 2.0 M KOH electrolyte. As shown in Fig. 4c, after 10[thin space (1/6-em)]000 cycles of charge and discharge at 1.0 A g−1, the specific capacitance retention rates for both CNFM electrodes are nearly 100%, indicating excellent cycling stability of the CNFMs. The GCD curves of the CNFM-20 electrode at the 1st and the 10[thin space (1/6-em)]000th cycle are shown in Fig. S7. Overall, the electrochemical characterization results show that CNFM-20 is an excellent electrode material for supercapacitor. The hierarchical pore structures provide a larger specific surface area for CNFM-20, which leads to the adsorption of more ions in the electrode; the interconnected fibrous structure and excellent conductivity also accelerate the transport of electrons. As a result, the synergistic effect of larger specific surface area, interconnected fibrous structure and excellent conductivity leads to high specific capacitance during charge and discharge process for the CNFM-20 electrode. Table S1 summarizes the surface properties and the supercapacitor performance of the electrospun CNFMs reported in recent years. In comparison with CNFMs prepared by other methods, the CNFMs prepared by carbonization of electrospun PSF/PAN nanofibrous mat in our work show superior surface properties and EDLC performance. Additionally, the PSF/PAN-derived CNFM-20 does not require post-preparation activation, while most of the methods in the literature require activation to form large surface areas and pores.

To further understand the electronic and ion transport in CNFMs, EIS measurements are carried out. The Nyquist plots of CNFM-20 and CNFM-0 are shown in Fig. 4d. The result shows a typical behavior of EDLCs based on porous carbon electrode. As shown in the inset of Fig. 4d, the semicircle at high frequency represents the accessibility of the pores (micropores/mesopores) to the ions in the electrolyte (referred to as the charge transfer resistance, Rct),31,32 and the intercept at the real axis represents the equivalent series resistance (Rs), whereas the linear behavior at the low frequency reflects the ion diffusion and capacitive response (called Warburg resistance). The large slope of the linear region of CNFM-20 indicates lower ion diffusion resistance and better capacitive behavior in comparison with CNFM-0. The smaller semicircle in the Nyquist plot of CNFM-20 in comparison to that of CNFM-0 indicates smaller Rct in the CNFM-20 electrode, which can be attributed to the fact that the hierarchical pore structures of CNFM-20 result in better ion accessibility. Additionally, Rs of the CNFM-20 electrode is 0.8 Ω, which is smaller than Rs of the CNFM-0 electrode (2.2 Ω), in consistent with the better conductivity of CNFM-20. Furthermore, the frequency response of the CNFMs is explored from the Bode plots (as shown in Fig. S8), and the time constant t0, which is defined as 1/f0 and reflects how fast the electrode can be reversibly charged and discharged under the characteristic frequency f0 at −45° phase, can be calculated. The CNFM-20 electrode has a shorter time constant (t0 = 1.0 s) than the CNFM-0 electrode (t0 = 1.43 s), in consistent with a better rate handling ability of CNFM-20.

The excellent electrochemical performance of the CNFMs prepared by electrospinning and carbonization of PAN with polysulfone as a sacrificial polymer enables us to make two-electrode supercapacitor without carbon activation and electrode additives (e.g. PVDF and active carbon). The CV curves of the device (Fig. 5a) at a scan rate ranging from 10 mV s−1 to 500 mV s−1 have symmetric, rectangular shape; at a scan rate as high as 500 mV s−1, the CV curve remains its rectangular shape, indicating excellent capacitive performance. Fig. 5b shows the GCD curves of the CNFM-20 based supercapacitor charged/discharged with different current density. The linear and symmetric GCD curves show that the CNFM-20 based device has excellent reversible behavior and ideal electric double-layer capacitive characteristics under fast charge/discharge. Additionally, the GCD curves with various charge/discharge rates have very small IR drop. Plot of the IR drop vs. current density in Fig. 5c shows a linear relationship, which can be fit based on the following eqn (2).33

 
IRdrop = a + bI (2)
here, a represents the difference between the applied potential of 1.0 V and the charged potential of the capacitor, b represents twice the value of the internal resistance, and I (A) is the discharge current. The small values of a and b for the linear fitting in Fig. 5c is consistent with the good performance of the device, which may be attributed to the hierarchically porous and interconnected structure of CNFM-20. The maximum power density (Pmax) of the device is calculated to be 30.7 kW kg−1 by the following eqn (3).33
 
image file: c8ra05957h-t2.tif(3)
where V0 (V) is the practical working potential of the supercapacitor device.


image file: c8ra05957h-f5.tif
Fig. 5 (a) CV curves of the two-electrode supercapacitor based on the freestanding CNFM-20 nanofibrous mat. (b) GCD curves of the CNFM-20 based device at current densities ranging from 0.25 A g−1 to 5 A g−1 (c) IR drop of the device vs. the current density. (d) The Ragone plot of energy density and power density of the CNFM-20 based supercapacitor.

Fig. 5d shows the Ragone plot of energy density and power density of the CNFM-20 based supercapacitor. The power density (P) (W kg−1) and the energy density (E) (W h kg−1) of a supercapacitor are calculated using following eqn (4)–(6):30

 
image file: c8ra05957h-t3.tif(4)
 
image file: c8ra05957h-t4.tif(5)
 
image file: c8ra05957h-t5.tif(6)
where Cm (F g−1) is the specific capacitance of device, ΔV (V) is the potential change within the discharge time Δt (s), M (g) is the mass of the active materials in the two electrodes, and I (A) is the set current of the GCD measurement. The energy density decreases with increase of power density. The supercapacitor device based on the CNFM-20 electrodes has the maximum energy density of 11.5 W h kg−1 and maximum power density of 2.49 kW kg−1. These values are comparable with those of supercapacitors based on carbon nanomaterials.34

4. Conclusion

In conclusion, carbon nanofibrous mats with high surface areas, hierarchical porous structures, and interconnected fibrous network are prepared by carbonization of electrospun nanofibers of PAN and PSF blend. The rapid degradation of PSF between 500 to 600 °C accompanied by release of SO2 gas results in formation of micropores and mesopores. Softened PSF at temperatures above the pre-oxidation (280 °C) and the high carbon residue after PSF degradation facilitate formation of interconnected junctions in the nanofibrous mat during carbonization of PSF/PAN. Additionally, the amount of graphitic carbon in the PSF/PAN based carbon nanofibrous mat increases in comparison to that in the PAN based carbon nanofibrous mat. These desired structural properties lead to high conductivity and excellent electrochemical performance of the PSF/PAN based carbon nanofibrous mat for supercapacitor electrode. The electrode from the PSF/PAN based carbon nanofibrous mat shows a specific capacitance of 272 F g−1 at current density of 1 A g−1, excellent cycling durability (100% capacitance retention after 10[thin space (1/6-em)]000 cycles), and good rate retention at current density of 50 A g−1.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work is supported by the National Natural Science Foundation of China (Grant Number 51573136), the Natural Science Foundation of Tianjin (Grant Number 15JCYBJC17800), and the Science and Technology Plans of Tianjin (Grant Number 16PTSYJC00110).

Notes and references

  1. M. Winter and R. J. Brodd, Chem. Rev., 2004, 104, 4245–4270 CrossRef PubMed.
  2. P. Simon and Y. Gogotsi, Nat. Mater., 2008, 7, 845–854 CrossRef PubMed.
  3. G. Wang, L. Zhang and J. Zhang, Chem. Soc. Rev., 2012, 41, 797–828 RSC.
  4. A. Borenstein, O. Hanna, R. Attias, S. Luski, T. Brousse and D. Aurbach, J. Mater. Chem. A, 2017, 5, 12653–12672 RSC.
  5. F. Wang, X. Wu, X. Yuan, Z. Liu, Y. Zhang, L. Fu, Y. Zhu, Q. Zhou, Y. Wu and W. Huang, Chem. Soc. Rev., 2017, 46, 6816–6854 RSC.
  6. C. Lai, Z. Zhou, L. Zhang, X. Wang, Q. Zhou, Y. Zhao, Y. Wang, X.-F. Wu, Z. Zhu and H. Fong, J. Power Sources, 2014, 247, 134–141 CrossRef.
  7. X. Lu, C. Wang, F. Favier and N. Pinna, Adv. Energy Mater., 2017, 7, 1601301 CrossRef.
  8. B.-H. Kim, K. S. Yang and J. P. Ferraris, Electrochim. Acta, 2012, 75, 325–331 CrossRef.
  9. L. Zhang, A. Aboagye, A. Kelkar, C. Lai and H. Fong, J. Mater. Sci., 2014, 49, 463–480 CrossRef.
  10. C. Kim and K. S. Yang, Appl. Phys. Lett., 2003, 83, 1216–1218 CrossRef.
  11. Y.-W. Ju, S.-H. Park, H.-R. Jung and W.-J. Lee, J. Electrochem. Soc., 2009, 156, A489–A494 CrossRef.
  12. T. Le, Y. Yang, Z. Huang and F. Kang, J. Power Sources, 2015, 278, 683–692 CrossRef.
  13. K. Huang, M. Li, Z. Chen, Y. Yao and X. Yang, Electrochim. Acta, 2015, 158, 306–313 CrossRef.
  14. N. C. Abeykoon, J. S. Bonso and J. P. Ferraris, RSC Adv., 2015, 5, 19865–19873 RSC.
  15. Y.-H. Hsu, C.-C. Lai, C.-L. Ho and C.-T. Lo, Electrochim. Acta, 2014, 127, 369–376 CrossRef.
  16. Y. Yao, K. K. Fu, S. Zhu, J. Dai, Y. Wang, G. Pastel, Y. Chen, T. Li, C. Wang, T. Li and L. Hu, Nano Lett., 2016, 16, 7282–7289 CrossRef PubMed.
  17. J. Ding, H. ping Zhang, X. Li, Y. Tang and G. Yang, Mater. Des., 2018, 141, 17–25 CrossRef.
  18. H. Wang, W. Wang, H. Wang, X. Jin, H. Niu, H. Wang, H. Zhou and T. Lin, ACS Appl. Energy Mater., 2018, 1, 431–439 CrossRef.
  19. Z. Zhou, C. Lai, L. Zhang, Y. Qian, H. Hou, D. H. Reneker and H. Fong, Polymer, 2009, 50, 2999–3006 CrossRef.
  20. M. Wu, Q. Wang, K. Li, Y. Wu and H. Liu, Polym. Degrad. Stab., 2012, 97, 1511–1519 CrossRef.
  21. A. M. Al-Enizi, A. A. Elzatahry, A. M. Abdullah, M. A. AlMaadeed, J. Wang, D. Zhao and S. Al-Deyab, Carbon, 2014, 71, 276–283 CrossRef.
  22. D. S. Knight and W. B. White, J. Mater. Res., 1989, 4, 385–393 CrossRef.
  23. Y.-X. Wang, C.-G. Wang, J.-W. Wu and M. Jing, J. Appl. Polym. Sci., 2007, 106, 1787–1792 CrossRef.
  24. https://www.solvay.com/en/markets-and-products/featured-products/udel.html, (last accessed: February 4, 2018).
  25. M. Rahaman, A. Ismail and A. Mustafa, Polym. Degrad. Stab., 2007, 92, 1421–1432 CrossRef.
  26. P. Almén and I. Ericsson, Polym. Degrad. Stab., 1995, 50, 223–228 CrossRef.
  27. L. Perng, J. Polym. Sci., Part A: Polym. Chem., 2000, 38, 583–593 CrossRef.
  28. S. T. Ellison, A. P. Gies, D. M. Hercules and S. L. Morgan, Macromolecules, 2009, 42, 3005–3013 CrossRef.
  29. L. Qie, W. Chen, H. Xu, X. Xiong, Y. Jiang, F. Zou, X. Hu, Y. Xin, Z. Zhang and Y. Huang, Energy Environ. Sci., 2013, 6, 2497 RSC.
  30. S. Zhang and N. Pan, Adv. Energy Mater., 2014, 5, 1401401 CrossRef.
  31. J. Kang, J. Wen, S. H. Jayaram, X. Wang and S.-K. Chen, J. Power Sources, 2013, 234, 208–216 CrossRef.
  32. A. Allagui, T. J. Freeborn, A. S. Elwakil and B. J. Maundy, Sci. Rep., 2016, 6, 38568 CrossRef PubMed.
  33. A. Izadi-Najafabadi, S. Yasuda, K. Kobashi, T. Yamada, D. N. Futaba, H. Hatori, M. Yumura, S. Iijima and K. Hata, Adv. Mater., 2010, 22, E235–E241 CrossRef PubMed.
  34. T. Liu, F. Zhang, Y. Song and Y. Li, J. Mater. Chem. A, 2017, 5, 17705–17733 RSC.

Footnote

Electronic supplementary information (ESI) available: SEM images of precursor nanofibrous mats; pore size distribution; XPS, and DSC of carbon nanofibrous mats; GDC curves of carbon nanofibrous mats; comparison of supercapacitors based electrospun nanofibrous materials. See DOI: 10.1039/c8ra05957h

This journal is © The Royal Society of Chemistry 2018
Click here to see how this site uses Cookies. View our privacy policy here.