Dashen
Dong
ab,
Qianqian
Shi
ab,
Debabrata
Sikdar
c,
Yunmeng
Zhao
ab,
Yiyi
Liu
ab,
Runfang
Fu
ab,
Malin
Premaratne
d and
Wenlong
Cheng
*ab
aDepartment of Chemical Engineering, Monash University, Clayton 3800, Victoria, Australia. E-mail: wenlong.cheng@monash.edu
bThe Melbourne Centre for Nanofabrication, 151 Wellington Road, Clayton 3168, Victoria, Australia
cDepartment of Electronics and Electrical Engineering, Indian Institute of Technology Guwahati, Guwahati 781039, India
dAdvanced Computing and Simulation Laboratory (AχL), Department of Electrical and Computer Systems Engineering, Monash University, Clayton 3800, Victoria, Australia
First published on 19th February 2019
The ability to control the site-selective deposition of a noble metal with nanoscale accuracy is vital for the synthesis of well-defined heterogeneous core-shell bimetallic nanoparticles for various applications ranging from nanophotonics to catalysis. Here, precise site-specific Ag coating onto concave gold nanoarrows (GNAs) is reported by tuning the concentration of the surfactant – cetyltrimethylammonium chloride (CTAC). Three distinct nanocoating structures, namely, anisotropic coating, middle coating, and conformal coating are obtained, which are achieved under low, medium and high CTAC concentrations, respectively. The site-specific nanoscale coating on GNAs is proved by scanning transmission electron microscopy imaging in conjunction with the elemental mapping. The CTAC concentration-dependent, facet-specific passivation may be the cause for the three distinct nanoparticles obtained. The morphology differences resulted in discrete plasmonic features, and a linear relationship between the resonance peak and the CTAC concentration is found for the conformal-coated GNAs. We further fabricate free-standing monolayer nanosheets out of the three kinds of nanoparticles, which display strong shape-dependent SERS enhancements.
Conceptual insightsPrecise site-specific Ag coating onto concave gold nanoarrows is demonstrated by virtue of fine-tuning the concentration of the surfactant – cetyltrimethylammonium chloride (CTAC). This enables anisotropic coating, middle coating, and conformal coating, as experimentally proved by scanning transmission electron microscopy imaging in conjunction with the elemental mapping and plasmonic profiles. Using the three kinds of nanoparticles obtained, we fabricate free-standing monolayered nanosheets with SERS enhancements highly dependent on the structures of the constituent building blocks. Our strategies represent a novel route to synthesize well-defined heterogeneous core–shell bimetallic nanoparticles for a myriad of potential applications in next-generation optoelectronics. |
Past decades have witnessed intensive research efforts to synthesize structurally well-defined bimetallic nanoparticles by controlling various parameters of seed-mediated growth. The types and amount of precursors added were found to relate to the asymmetric structures of core–shell nanocrystals.12,13 By adjusting the pH, the deposition could also be controlled on either end or in the middle of elongated particles.14 Dendritic nanocrystals could be obtained through a co-reduction process where the surface diffusion was slowed down by controlling the relative amount of reducing agents.15–18 Besides, templates, such as silica, were used as a protective layer to ensure site-specific growth on the exposed particle surfaces, leading to asymmetric bimetallic particles.19–21 Capping agents were recently found to play key roles in shape control because of their facet-specific binding properties. For example, the controlled deposition of Ag on Pd nanocubes was achieved by using poly(vinyl pyrrolidone).22
Here, we report a highly efficient surfactant-based approach to site-specifically control Ag coating on concave gold nanoarrows (GNAs) simply by tuning the concentration of cetyltrimethylammonium chloride (CTAC). Under a low CTAC concentration, Ag deposition on GNA was non-uniform, leading to a cuboid-shaped shell, which is termed anisotropic coating (ac-GNA); when the CTAC concentration is in the middle range, Ag would selectively deposit onto the concave part of the GNA, which is termed selective middle coating (mc-GNA); at a high CTAC concentration, Ag would deposit conformally across the entire surface of GNA, which is termed conformal coating (cc-GNA). The three distinct coating structures were confirmed by high-resolution electron microscopy in conjunction with elemental mapping, and are also in excellent agreement with the characteristic plasmonic resonance spectra observed. CTAC concentration-dependent, facet-specific passivation may be the cause of the site-specific Ag deposition described above. We further fabricated nanosheets using our two-step drying-mediated self-assembly,23 which exhibited strong coating-dependent surface enhanced Raman scattering (SERS).
To deposit Ag onto the GNAs, the GNA particles were first re-dispersed in CTAC solutions with three different concentrations (80, 378 and 600 mM). Then, AgNO3 and ascorbic acid were added in sequence under constant stirring in a 60 °C water bath. The reaction was kept for 4 hours. This process led to the reduction of silver ions and consequent deposition on the GNA surfaces. To fully understand how the surfactants influenced the silver coating, all other experimental conditions were identical except for varying the surfactant concentration.
The coating of Ag onto GNA was carefully characterized by electron microscopy. Transmission electron microscopy (TEM) images of Ag coated GNA show that the Ag coating process was highly dependent on the CTAC concentration (Fig. 1a). The cuboid-shaped nanoparticles, nanoarrows with smooth surface in the middle and nanoarrows with concave surface in the middle were clearly observed for low, middle and high concentration of CTAC. All of these particles turned out to be single crystals as demonstrated from the selective area electron diffraction (SAED) pattern (Fig. S2, ESI†). These SAED patterns matched well with face-centered-cubic silver.
To further reveal where silver coating occurred, we conducted a characterization using STEM-HAADF (high-angle annular dark-field) and STEM-EDS (energy-dispersive X-ray spectroscopy). Fig. 1b–d presents the STEM-HAADF images and their corresponding elemental maps. Good contrast of the Au core and Ag shell components could be clearly seen on all the HAADF images and the EDS maps gave the distribution information of Au and Ag elements. Under low CTAC concentration, the GNA core was fully covered with cuboid shaped Ag shell. Because the coating was not uniform across the GNA surface, it was termed as ac-GNA to reflect the anisotropic-coated GNA (Fig. 1b). When the CTAC concentration was in the middle range, most of the Ag element was deposited on the middle shaft rather than the two pyramid heads of the GNA and these middle coating only nanoparticles were called mc-GNAs (Fig. 1c). When the CTAC concentration was high, a continuous conformal Ag layer was found across the GNA surface, which was termed as conformally coated GNA (cc-GNA), as shown in Fig. 1d. The three distinct Ag coatings on the GNAs were highly reproducible and could be seen in a large-scale elemental mapping as shown in Fig. S3 (ESI†).
Corresponding to the three distinct particle structures, we observed the corresponding optical properties. A yellow, red and dark purple solution was obtained for 80 mM, 378 mM and 600 mM CTAC, respectively (Fig. 2a), which refers to ac-GNA, mc-GNA and cc-GNA. Corresponding to these visual colors, three distinct plasmonic spectra were observed, as shown in Fig. 2b. For the GNA solution, there were two resonance peaks located at 539 nm and 666 nm, corresponding to the dipolar transverse and longitudinal modes, respectively. For ac-GNA (80 mM CTAC), there were four resonance peaks, the two on the left corresponding to the longitudinal and transverse dipolar plasmon modes, while the two on the right were attributed to the octupolar modes, which is similar to the Au@Ag cuboid shell particles.26 For mc-GNA (378 mM CTAC), we also found four resonance peaks. In comparison with the cuboid shell one, there was an obvious red shift for the transverse dipolar mode, which was due to less Ag deposition, in excellent agreement with the TEM and elemental mapping results (Fig. 1c). Consistently, the absence of silver deposition in the GNA pyramid ends led to a slight longitudinal dipolar mode blue shift. This was also in agreement with the electric-field distribution as shown in Fig. 2c. As for the cc-GNAs (600 mM CTAC), the line shape resembled that for the original GNAs except for the two resonance peaks blue shifting to ∼516 nm and ∼582 nm. Simultaneously, an additional peak at 343 nm was observed. This correlates very well with the thin conformal Ag coating on the GNAs (Fig. 1d). We also carried out a simulation study to trace the spectral changes with different silver coatings onto GNAs (Fig. 2d). Here, to make simulations less computationally expensive, we built simulation models based on a few simplifying assumptions; they possess symmetry (Fig. S4, ESI†), whereas samples are more complex geometrically. Nevertheless, qualitatively our models produce results exhibiting trends similar to those seen from experiments.
To reveal how CTAC could induce such site-specific coating, we fine-tuned the experimental conditions with eight different CTAC concentrations, from 80 mM to 756 mM. As shown in the TEM images (Fig. S5, ESI†), a transition from homogeneous Ag cuboid shaped shell to heterogeneous concave site-specific Ag deposition could be clearly seen when the CTAC concentration is increased from 80 mM (low) to 378 mM (medium). Since CTAC has no covalent bonding with the nanoparticles, the absorbed CTAC must be in dynamic chemical equilibrium with that present in bulk solution. The more CTAC molecules are present in the bulk solution, the more likely they absorb onto the nanoparticle surfaces. Under 80 mM CTAC, CTAC molecules might loosely pack on the GNA surfaces (Fig. S6 left, ESI†). This enabled the facile penetration of Ag ions and ascorbic acids into the CTAC capping layers. In this condition, the rapid nucleation and growth led to the formation of cuboid-shaped silver, similar to the case of gold nanorods.26 When the CTAC concentration was further increased, CTAC would likely form a denser bilayer on the GNA surface. Different from cetyltrimethylammonium bromide (CTAB),27,28 it has been reported that the CTAC has a similar affinity with Au [111] (pyramid heads of GNA) and [110] (middle shaft of GNA) facets.29 However, due to the curvature effect,30,31 a non-compact bilayer would likely form in the middle shaft of GNA (Fig. S6 middle, ESI†). In this situation, the Ag deposition occurs on the middle concave shaft parts. When the CTAC centration was further increased (high, >500 mM), densely packed layers eventually also formed in the middle concave areas. These conformal densely packed CTAC molecules might form bilayers,32 which shielded the GNA surfaces from the effective access of silver ions and ascorbic acid. Hence, only a thin Ag deposition was possible. Our 1H NMR results also showed significant differences of CTAC mass attached on the freeze-dried GNA surfaces under different concentrations of the CTAC aqueous solution, which supports our argument on the concentration-dependent distribution of CTAC on GNA (Fig. S7, ESI†).
To further prove the above mechanism, we investigated how the CTAC concentration influenced the silver coating in the high concentration regime (>500 mM). The colors of the nanoparticle solutions were found to change from dark red to dark blue when the CTAC concertation was increased from 500 mM to 750 mM (Fig. 3a). The corresponding plasmonic resonance spectra were recorded as shown in Fig. 3b. As expected, all the samples should be cc-GNA with two resonance peaks corresponding to dipolar transverse modes (peak I indicated by the grey color) and dipolar longitudinal modes (peak II indicated by red color). At the higher CTAC concentration, both peaks shifted to the red region, moving closer to the peaks of the original GNAs. Moreover, the small peak that appeared at around 340 nm for the 500 mM CTAC sample gradually disappeared with increased concentration. These phenomena proved our argument that denser CTAC layers will build up around the GNAs making the Ag deposition less favorable. This explained well the gradual disappearance of the characteristic Ag peak at 340 nm and accompanying closer peak matching to the original GNAs. Interestingly, we found a linear relationship between the resonance peak position and the CTAC concentration for both peaks I and II after multiple tests (Fig. 3c and d). The fitting led to the following equation:
yI = 503.370 + 0.02x | (1) |
yII = 541.359 + 0.07x | (2) |
We further used the GNAs, ac-GNAs, mc-GNAs and cc-GNAs as building blocks to fabricate monolayer nanosheets by using our recently developed two-step drying-mediated self-assembly approach.23 After functionalizing the nanoparticles with thiol-terminated polystyrene (PS), they became hydrophobic and could self-assemble at the air–water interface (Fig. S8, ESI†). Upon water evaporation, two-dimensional superlattice nanosheets were obtained on the silicon wafers. The well-ordered horizontal aligned monolayer structure of the nanoparticles could be clearly seen in Fig. 4a–d. The 2D orientational order (S2D) was calculated to be around 0.73, 0.78, and 0.75 respectively for the ac-GNA, mc-GNA and cc-GNA nanosheets after choosing three random regions for each sample (Fig. S9, ESI†). Vertical alignments of those particles within the superlattices were also found in some regions as shown in Fig. S10 (ESI†).
Our previous work has shown that the two-dimensional superlattice nanosheets could serve as a new class of SERS substrate.6,8 Therefore, we investigated the SERS performance of the obtained nanosheets by using 4-aminothiolphenol (4-ATP) as the Raman dye. The nanosheets were first subjected to a short time UV-Ozone treatment and then immersed into a 10 μM 4-ATP ethanol solution. The morphology of the particles was checked before and after treatment to ensure that there was no influence on the structure integrity (Fig. S11, ESI†). Then the nanosheets were placed into a confocal micro-Raman system after being rinsed with ethanol. The excitation laser was chosen as 633 nm which was close to the resonance peak of the fabricated nanosheets33 (Fig. S12, ESI†). As shown in Fig. 4e, the fingerprint peaks of 4-ATP at 1078 and 1578 cm−1 are evident, which are due to the dominated enhancement of a1 vibrational modes, ν(C–S) and ν(C–C), respectively. Among the three Ag-coated nanoparticles, the ac-GNA nanosheet showed the highest Raman intensity, while the cc-GNA showed the lowest intensity. This can be explained by the amount of Ag coated onto the GNA since the extinction coefficient of silver is much higher than that of gold.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c8nh00431e |
This journal is © The Royal Society of Chemistry 2019 |