Poly(ethylene oxide)/Ag ions and nanoparticles/1-hexyl-3-methylimidazolium tetrafluoroborate composite membranes with long-term stability for olefin/paraffin separation

Hyunsik Jeona and Sang Wook Kang*ab
aDepartment of Chemistry, Sangmyung University, Seoul 03016, Republic of Korea. E-mail: swkang@smu.ac.kr; Fax: +82 2 2287 5362; Tel: +82 2 2287 5362
bDepartment of Chemistry and Energy Engineering, Sangmyung University, Seoul 03016, Republic of Korea

Received 9th November 2018 , Accepted 26th January 2019

First published on 6th February 2019


Abstract

A poly(ethylene oxide)(PEO)/AgBF4/1-hexyl-3-methylimidazolium tetrafluoroborate (HMIM+BF4) composite membrane that exhibits long-term stability was prepared for olefin/paraffin separation. The membrane was prepared by simply adding AgBF4 and HMIM+BF4 to a solution of PEO. Long-term stability testing showed that the separation performance of the membrane is maintained for ≈100 h owing to the Ag NPs formed in the membrane, which are olefin carriers, being stabilized by HMIM+BF4. In terms of separation performance, the PEO/AgBF4/HMIM+BF4 composite membrane exhibited a propylene/propane selectivity of 11.8 and a mixed-gas permeance of 11.3 GPU. We also investigated the factors that determine separation performance by comparison with a PEO/AgBF4/1-butyl-3-methylimidazolium tetrafluoroborate (BMIM+BF4) composite membrane. The PEO/AgBF4/HMIM+BF4 composite membrane was characterized by scanning electron microscopy, FT-IR spectroscopy, ultraviolet-visible spectroscopy, thermogravimetric analysis, and Raman spectroscopy.


I. Introduction

Olefins, commonly known as alkenes, are hydrocarbons with carbon–carbon double bonds, while paraffin, known as alkanes, are hydrocarbons having only single bonds.1 Light olefins, such as ethylene and propylene, are key monomers in petrochemical and polymer synthesis.2 Thus, olefins are used to produce many other organic chemicals. In 2011, 141 million tons of ethylene were produced worldwide.3,4 Most olefins are produced by steam cracking of naphtha, propane, and light oil. However, this process produces a mixture of olefins and paraffin.5 Therefore, the separation of olefins from olefin/paraffin mixtures is very important in the petrochemical industry.6–8 The separation of olefin/paraffin mixtures is most commonly performed by cryogenic distillation because of the similar properties of olefins and paraffin.9–11 However, this process suffers from the disadvantages of requiring considerable capital input and being energy intensive.12 In order to overcome these problems, membrane separation has emerged as a simple, low-energy manufacturing process.13,14 However, while glassy polymer membranes show high selectivity, they typically exhibit low permeability. Conversely, rubbery polymers exhibit high permeability but poor selectivity.15 Recently, facilitated transport membranes, which are selectively permeable to only specific substances, have been attracting research attention.10 Facilitated transport, which exploits the concentration gradient of solutes generated by the reversible reactions of compounds in membrane with specific solutes, promotes the transport of these solutes.16 For example, a dimethylpropylenediamine ethoxyacetate ([DMAPAH][EOAc]) membrane for CO2/N2 separation using diamine-monocarboxylate protic ionic liquids (PILs) as carriers has been reported to show a selectivity of 151 and a CO2 permeability of 3028 barrer.17 In addition, an arginine salt-chitosan membrane using the amino group in the arginine salt as a carrier was reported to show a selectivity of 144 and a CO2 permeability of 1500 barrer in CO2/H2 separation.18 Recently, it has been reported that PEBAX-1657, which is a permeable polymer that contains Ag ions as olefin carriers, has a propylene/propane selectivity of 8.8 and a permeability of 22.5 GPU.19 In general, Ag salts are used as olefin carriers, but Ag ions generated from Ag salts are easily reduced and consequently lose carrier activity.20–22 Thus, attempts have been made to partially polarize the surface of Ag NPs so that they react reversibly with olefins.21 However, Ag NPs acting as olefin carriers have a drawback in that the permeability of the host membrane is lowered due to the barrier action that occurs when the Ag NPs aggregate to form larger NPs.22 In addition, membranes using ZIF and MOF have also been reported.23–32 Recently, we fabricated a poly(ethylene oxide)(PEO)/AgBF4/1-butyl-3-methylimidazolium tetrafluoroborate (BMIM+BF4) composite membrane in an attempt to restrict the size of the Ag NPs formed therein. We reasoned that BMIM+BF4 would stabilize the smaller nascent Ag NPs, inhibiting their aggregation and thus maintaining membrane permeability. The average size of the particles formed in the composite membrane after the long-term test was 4.55 nm. The prepared PEO/AgBF4/BMIM+BF4 composite membrane exhibited a propylene/propane selectivity of ≈15 and a permeability of 12 GPU.33 In the current study, we assessed whether stability could be maintained using ionic liquids other than BMIM+BF4 in order to investigate the factors that contribute to the long-term stability of such membranes. 1-Hexyl-3-methylimidazolium tetrafluoroborate (HMIM+BF4) was used as the new ionic liquid to investigate the effect of the carbon chain length of ionic liquids, and compared with BMIM+BF4 in viewpoint of both stabilizing the nanoparticles and separation performance.

II. Experimental

2.1. Materials

Acetonitrile (99.8%) was purchased from Aldrich Chemical Co. and PEO (Mw 6 × 105 g mol−1) was purchased from ACROS Co. Silver tetrafluoroborate (AgBF4, 98%) was purchased from Tokyo Chemical Industry Co., and HMIM+BF4 was purchased from C-TRI. The microporous polysulfone support was provided by Toray Chemical Inc., Korea. All the initial solvents and materials were used without further purification.

2.2. Characterization

Scanning electron microscopy (SEM) images were obtained using JEOL JSM-5600LV. The weight loss of the complex was measured using thermogravimetric analysis (TGA, TGA Q50, TA Instruments) under N2 flow. The ultraviolet-visible (UV-Vis) absorption spectra were recorded using a Beckman Coulter Life Sciences DU 730 Life Science UV-Vis spectrophotometer with 1 nm resolution. The IR measurements were performed on a VERTEX 70 FT-IR spectrometer; 16–32 scans were signal averaged with a resolution of 8 cm−1. Raman spectra of neat HMIM+BF4 were obtained using a BRUKER RAM II instrument at a resolution of 0.5 cm−1.

2.3. Membrane preparation

The PEO/AgBF4/HMIM+BF4 complex membrane was prepared by adding AgBF4 and HMIM+BF4 to a PEO polymer solution and vacuum drying. The 5 wt% PEO polymer solution was prepared by dissolving PEO in water/acetonitrile (9[thin space (1/6-em)]:[thin space (1/6-em)]10 w/w). AgBF4 was added to the prepared PEO polymer solution at 1[thin space (1/6-em)]:[thin space (1/6-em)]1 molar ratio, and HMIM+BF4 was added at different mole ratios. The solution was coated onto polysulfone microporous membrane supports using an RK Control Coater (Model K202, Control Coater RK Print-Coat Instruments Ltd., UK). The long-term stability of the composite membrane prepared at a composition of 1/1/0.052 and vacuum dried for 24 h showed the best performance.

2.4. Gas separation performance

The permeation test was performed by permeating the PEO/AgBF4/HMIM+BF4 composite membrane with a propylene/propane mixed gas (1[thin space (1/6-em)]:[thin space (1/6-em)]1 v/v). The permeance was measured using a bubble flow meter and the selectivity was assessed by gas chromatography (YoungLin 6500 GC system). The flow rate of the mixed gas was controlled by a mass flow controller (MFC). The unit of gas permeance is GPU (1 GPU = 1 × 10−6 cm3 (STP)/(cm2 s cmHg)).

III. Results and discussion

3.1. SEM images

Fig. 1 shows a cross-section of the PEO/AgBF4/HMIM+BF4 composite membrane. The membrane was prepared by coating PEO/AgBF4/HMIM+BF4 solution onto a polysulfone support and vacuum drying for 24 h. The sponge-like polysulfone support was well coated with PEO/AgBF4/HMIM+BF4. The thickness of the resultant layer was ≈4.5 μm.
image file: c8ra09274e-f1.tif
Fig. 1 Cross-sectional SEM image of PEO/AgBF4/HMIM+BF4 composite membrane.

3.2. UV-Vis absorption spectra

The stabilizing effect of HMIM+BF4 on the Ag NPs generated in PEO/AgBF4/HMIM+BF4 solution was investigated by UV-Vis spectroscopy. PEO/AgBF4/HMIM+BF4 solutions were heated at 70 °C for 10, 20, 30, and 60 min. The peak for Ag NPs is typically observed at 420 nm.21 Thus, a peak at about 420 nm indicates the formation of Ag NPs, while the intensity of the peak represents the concentration of Ag NPs formed. When the PEO/AgBF4/HMIM+BF4 solution is heated for 10 min, a peak is observed at 403–423 nm. Upon heating for 20 min, a slight peak shift is observed. Upon heating for 30 and 60 min, no further peak shifting is observed, but the peak intensity increases. These results indicate that Ag NPs are stabilized by HMIM+BF4. This is because the surface of the Ag NPs is partially polarized by HMIM+BF4, thus inhibiting aggregation and particle growth. As a result, after a heating time of 20 min, only small Ag NPs are formed. Moreover, the spectrum presents a symmetric peak, indicating that monodisperse AgNPs were formed in the PEO/AgBF4/HMIM+BF4 solution. From these results, it was confirmed the effect of stabilizing the NPs by ILs since the relatively narrow peak was observed at UV-Vis spectroscopy (Fig. 2).
image file: c8ra09274e-f2.tif
Fig. 2 UV-Vis absorption spectra of PEO/AgBF4/HMIM+BF4 solution with heating time.

3.3. FT-IR spectra

FT-IR was measured to confirm the coordination interactions of ether group and Ag ion of PEO. Fig. 3 showed the ether group stretching band peak of PEO/AgBF4/HMIM+BF4 complex. Generally, the ether group stretching band peak of neat PEO was known to be observed at 1082 cm−1. When AgBF4 was incorporated into PEO, the peak shifted to about 1070 cm−1. This was attributable to the interaction between the Ag ion and oxygen in ether group resulting in weaker C–O bonds.34 Furthermore, when HMIM+BF4 was additionally inserted into PEO/AgBF4 complex, the peak shifted to 1014 cm−1. This could be explained by the interaction of HMIM+ with BF4 of AgBF4, resulting in the weakened bond between Ag ions and BF4, and the strong interaction between Ag+ and oxygen in ether group. Therefore, the C–O bond became weakened and free BF4 of HMIM+BF4 could stabilize the generated Ag NPs.
image file: c8ra09274e-f3.tif
Fig. 3 FT-IR spectra of PEO/AgBF4/HMIM+BF4 complex.

3.4. Separation performance for propylene/propane mixtures

Fig. 4 shows the propylene/propane separation performance of the PEO/AgBF4/HMIM+BF4 composite membrane. The selectivity is initially 8.1 and then increases slightly after 20 h, remaining at ≈11.8 for 100 h. The permeance decreases with the evaporation of the solvent remaining in the membrane, but the rate of decrease slows after 50 h and the permeance remains at 11.3 GPU at 100 h. This separation performance is due to the stabilization of the Ag NPs by HMIM+BF4. The Ag NPs formed in the PEO/AgBF4/HMIM+BF4 composite membrane are stabilized by HMIM+BF4, inhibiting their aggregation. Smaller Ag NPs act as more efficient olefin carriers; thus, the propylene/propane separation performance of the PEO/AgBF4/HMIM+BF4 composite membrane is maintained because the NPs do not aggregate as shown in Scheme 1.
image file: c8ra09274e-f4.tif
Fig. 4 Separation performance of PEO/AgBF4/HMIM+BF4 composite membrane. (a) Selectivity for propylene/propane mixture, and (b) mixed gas permeance.

image file: c8ra09274e-s1.tif
Scheme 1 Ag NPs formation in PEO/AgBF4/HMIM+BF4 composite membrane upon heating.

3.5. Thermogravimetric analysis

The thermal stabilities of neat PEO, PEO/AgBF4, and PEO/AgBF4/HMIM+BF4 membranes were measured by TGA. Fig. 5 shows the weight loss for each membrane at temperatures ranging from room temperature to 700 °C. For the neat PEO membrane, a large weight loss occurs between 380 and 450 °C owing to the degradation of the polymer. The PEO/AgBF4 and PEO/AgBF4/HMIM+BF4 membranes exhibit weight losses at lower temperatures owing to the interaction between the added AgBF4 and the PEO chains. Furthermore, when HMIM+BF4 was added to PEO/AgBF4, there was significant change in the curve compared to that for PEO/AgBF4, indicating that plasticizing effect is produced by the added HMIM+BF4. This result was same from that for the PEO/AgBF4/BMIM+BF4 composite membrane previously reported. The TGA of PEO/AgBF4/BMIM+BF4 composite membrane was measured in the presence of polysulfone support, but was plasticized like the PEO/AgBF4/HMIM+BF4 membrane.33 Due to this plasticizing effect, the permeance does not decrease due to the generation of nanoparticles but the permeance remains constant.
image file: c8ra09274e-f5.tif
Fig. 5 TGA curves for neat PEO (red), PEO/AgBF4 (blue), and PEO/AgBF4/HMIM+BF4 (green) complex.

Raman spectra were obtained to investigate the state of BF4 in HMIM+BF4. In general, the free ion, ion pair, and ion aggregate stretching bands of BF4 are observed at 765, 770, and 774 cm−1, respectively.35 In previous studies, the BF4 ionic constituents of neat BMIM+BF4 were found to exist mostly as ion pairs with some ion aggregates.36 However, the BF4 ionic constituents of neat HMIM+BF4 are mainly observed to be free ions (740 cm−1), as shown in Fig. 6. In general, the more of the ionic liquid that exists as free ions, the better its ability to stabilize Ag NPs. Thus, HMIM+BF4 stabilizes Ag NPs more than BMIM+BF4, but HMIM+BF4 has low molecular mobility because of its large molecular size and thus initially does not stabilize Ag NPs. Therefore, slightly larger Ag NPs are initially formed in HMIM+BF4. In addition, HMIM+BF4 molecules do not exhibit good mobility even when they penetrate the polymer, because of their large size. This is consistent with the fact that the plasticizing effect does not occur.


image file: c8ra09274e-f6.tif
Fig. 6 Raman spectrum of neat HMIM+BF4.

Therefore, the PEO/AgBF4/HMIM+BF4 composite membrane exhibits poorer performance than that of the PEO/AgBF4/BMIM+BF4 composite membrane owing to the increased size of the initially formed Ag NPs and the low mobility of HMIM+BF4 in the polymer. The separation performances of the PEO/AgBF4/HMIM+BF4 composite membranes were compared in Table 1.

Table 1 Propylene/propane selectivity and mixed-gas permeance of PEO/AgBF4/HMIM+BF4 composite membranes after conversion of Ag ions to Ag nanoparticles
  Selectivity (propylene/propane) Permeance (GPU)
PEO/AgBF4/HMIM+BF4 composite membrane 11.8 11.3


IV. Conclusions

We succeeded in preparing for the PEO/AgBF4/HMIM+BF4 composite membrane and confirmed the long-term stability of propylene/propane selectivity of 11.8 and permeance of 11.3 GPU for more than 100 h. The long-term stability is owing to the stabilization of the Ag NPs by ionic liquid HMIM+BF4. HMIM+BF4 could partially polarize the surfaces of Ag NPs generated under separation process, resulting in the formation of olefin carriers. We also compared the performance of the PEO/AgBF4/BMIM+BF4 composite membrane with that of the current membrane to help elucidate the factors that determine separation performance in such membranes. As a result, the effect of the carbon chain length of ionic liquids was investigated, and both butyl in BMIM+BF4 and hexyl groups in HMIM+BF4 were found to be effective in stabilizing the nanoparticles. However, by identifying other ionic liquids with longer carbon chains such as 1-methyl-3-octylimidazolium tetrafluoroborate in the future, we intend to identify main factors in the design of long-term stable facilitated olefin transport membranes.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was supported by the Basic Science Research Program (2017R1D1A1B03032583) through the National Research Foundation of Korea (NRF), funded by the Ministry of Science, ICT, and Future Planning. This study was also funded by Korea Environment Industry & Technology Institute (KEITI) as “Technology Program for establishing biocide safety management”. (RE201805019).

Notes and references

  1. C. H. Park, J. H. Lee, J. P. Jung and J. H. Kim, J. Membr. Sci., 2017, 533, 48–56 CrossRef CAS .
  2. W. J. Koros, AIChE J., 2004, 50, 2326–2334 CrossRef CAS .
  3. S. Jeong and S. W. Kang, Chem. Eng. J., 2017, 327, 500–504 CrossRef CAS .
  4. W. R. True, Oil Gas J., 2012, 110, 78–84 Search PubMed .
  5. R. B. Eldridge, Ind. Eng. Chem. Res., 1993, 32, 2208–2212 CrossRef .
  6. R. L. Burns and W. J. Koros, J. Membr. Sci., 2003, 211, 299–309 CrossRef CAS .
  7. D. J. Safarik and R. B. Eldridge, Ind. Eng. Chem. Res., 1998, 37, 2571–2581 CrossRef CAS .
  8. M. Azhin, T. Kaghazchi and M. Rahmani, J. Ind. Eng. Chem., 2008, 14, 622–638 CrossRef CAS .
  9. T. Ren, M. Patel and K. Blok, Energy, 2006, 31, 425–451 CrossRef CAS .
  10. S. J. Kim, J. P. Jung, C. H. Park and J. H. Kim, Membr. J., 2015, 25, 496–502 CrossRef .
  11. R. Faiz and K. Li, Chem. Eng. Sci., 2012, 73, 261–284 CrossRef CAS .
  12. J. H. Kim, S. W. Kang and Y. S. Kang, J. Polym. Res., 2012, 19, 9753–9759 CrossRef .
  13. S. M. Davoodi, M. Sadeghi, M. Naghsh and A. Moheb, RSC Adv., 2016, 6, 23746–23759 RSC .
  14. O. Salinas, X. Ma, E. Litwiller and I. Pinnau, J. Membr. Sci., 2016, 500, 115–123 CrossRef CAS .
  15. B. D. Freeman, Macromolecules, 1999, 32, 375–380 CrossRef CAS .
  16. I. S. Chae, S. W. Kang and Y. S. Kang, RSC Adv., 2014, 4, 30156–30161 RSC .
  17. X. M. Zhang, Z. H. Tu, H. Li, L. Li, Y. T. Wu and X. B. Hu, J. Membr. Sci., 2017, 527, 60–67 CrossRef CAS .
  18. L. A. El-Azzami and E. A. Grulke, J. Membr. Sci., 2009, 328, 15–22 CrossRef CAS .
  19. S. Jeong, H. Sohn and S. W. Kang, Chem. Eng. J., 2018, 333, 276–279 CrossRef CAS .
  20. S. W. Kang, W. Bae, J. H. Kim, J. H. Lee and Y. S. Kang, Ind. Eng. Chem. Res., 2009, 48, 8650–8654 CrossRef CAS .
  21. S. W. Kang and Y. S. Kang, J. Colloid Interface Sci., 2011, 353, 83–86 CrossRef CAS PubMed .
  22. I. S. Chae, S. W. Kang, J. Y. Park, Y. G. Lee, J. H. Lee, J. Won and Y. S. Kang, Angew. Chem., Int. Ed., 2011, 50, 2982–2985 CrossRef CAS PubMed .
  23. A. Luna-Triguero, J. M. Vicent-Luna, P. Gómez-Álvarez and S. Calero, J. Phys. Chem. C, 2017, 121, 3126–3132 CrossRef CAS .
  24. S. Bendt, M. Hovestadt, U. Böhme, C. Paula, M. Döpken, M. Hartmann and F. J. Keil, Eur. J. Inorg. Chem., 2016, 27, 4440–4449 CrossRef .
  25. U. Böhme, B. Barth, C. Paula, A. Kuhnt, W. Schwieger, A. Mundstock, J. Caro and M. Hartmann, Langmuir, 2013, 29, 8592–8600 CrossRef PubMed .
  26. K. Eum, C. Ma, A. Rownaghi, C. W. Jones and S. Nair, ACS Appl. Mater. Interfaces, 2016, 8, 25337–25342 CrossRef CAS PubMed .
  27. L. Xu, M. Rungta and W. J. Koros, J. Membr. Sci., 2011, 380, 138–147 CrossRef CAS .
  28. S. H. Kunjattu, V. Ashok, A. Bhaskar, K. Pandare, R. Banerjee and U. K. Kharul, J. Membr. Sci., 2018, 549, 38–45 CrossRef CAS .
  29. Y. H. Chu, D. Yancey, L. Xu, M. Martinez, M. Brayden and W. Koros, J. Membr. Sci., 2018, 548, 609–620 CrossRef CAS .
  30. M. J. Lee, M. R. Abdul Hamid, J. Lee, J. S. Kim, Y. M. Lee and H. K. Jeong, J. Membr. Sci., 2018, 559, 28–34 CrossRef CAS .
  31. J. Yu, C. Wang, L. Xiang, Y. Xu and Y. Pan, Chem. Eng. Sci., 2018, 179, 1–12 CrossRef CAS .
  32. V. F. D. Martins, A. M. Ribeiro, A. Ferreira, U. H. Lee, Y. K. Hwang, J. S. Chang, J. M. Loureiro and A. E. Rodrigues, Sep. Purif. Technol., 2015, 149, 445–456 CrossRef CAS .
  33. H. Jeon and S. W. Kang, Polym. Compos., 2018 DOI:10.1002/pc.25082 .
  34. K. W. Yoon, Y. S. Kang and S. W. Kang, J. Membr. Sci., 2016, 513, 95–100 CrossRef CAS .
  35. J. H. Lee, J. Hong, J. H. Kim, Y. S. Kang and S. W. Kang, Chem. Commun., 2012, 48, 5298–5300 RSC .
  36. D. Ji, Y. S. Kang and S. W. Kang, Sci. Rep., 2015, 5, 16362–16367 CrossRef CAS PubMed .

This journal is © The Royal Society of Chemistry 2019
Click here to see how this site uses Cookies. View our privacy policy here.