A graphite-modified natural stibnite mineral as a high-performance anode material for sodium-ion storage

Hongliang Lia, Mingxiang Deng*b, Hongshuai Hou*a and Xiaobo Jia
aCollege of Chemistry and Chemical Engineering, Central South University, Changsha, 410083, China. E-mail: hs-hou@csu.edu.cn; Fax: +86-731-88879616; Tel: +86-731-88877237
bCollege of Science, Central South University of Forestry and Technology, Changsha, 410004, China. E-mail: 511584588@qq.com

Received 9th April 2019 , Accepted 1st July 2019

First published on 17th September 2019


Abstract

Recently, Sb2S3 has drawn extensive interest in the energy storage domain due to its high theoretical capacity of 946 mA h g−1. However, the inherent disadvantages of serious volume expansion and poor conductivity restrict the development of Sb2S3 for its application in SIBs. In addition, chemical synthesis is a main method to prepare Sb2S3, which is commonly accompanied by environmental pollution and excessive energy consumption. Herein, the natural stibnite mineral was directly applied in SIBs after modification with graphite via an effective and facile approach. The novel composites exhibited excellent electrochemical properties with higher reversible capacity, better rate capability and more outstanding cycling stability than the bare natural stibnite mineral. Briefly, this study is anticipated to provide a reference for the development of natural minerals as first-hand materials in energy storage and a new approach to improve natural stibnite mineral composites for their application as anodes in SIBs.


1. Introduction

With the rapid growth of large-scale energy storage and electric vehicle market, the demand for rechargeable lithium-ion batteries (LIBs) is also continuously increasing. However, some barriers, including the limited and uneven distribution of lithium resources in the world, strictly hamper the further development of LIBs;1 in this regard, sodium-ion batteries (SIB) can be an effective supplementary artifice for LIBs in the large-scale energy storage domain owing to abundant sodium resources with even global distribution and similar electrochemical energy storage principles of SIBs to LIBs.2,3 However, the larger radius of sodium ions (0.102 nm) and the higher energy cost for the formation of graphite intercalation compounds as compared to the case of commercial graphite anode materials in LIBs hinder the application of SIBs. Some amorphous carbon materials, such as porous carbons, carbon tubes, carbon nanosheets, and doped carbons, have been confirmed to possess good sodium storage performances.4–8 Since the standard electrode potential of Na/Na+ (−2.71 V vs. SHE) is higher than that of Li/Li+ (−3.04 V vs. SHE) and the specific capacities of most carbon anode materials are less than 400 mA h g−1, these factors would limit the energy density of SIBs. Hence, it is significant to develop and design new materials with high capacity and long cycle life for SIBs.

Sb2S3 has gained widespread attention as an anode material for SIBs because of its high theoretical capacity of 946 mA h g−1 based on both the conversion reaction: Sb2S3 + 6Na+ +6e → 2Sb + 3Na2S, and the alloying reaction: 2Sb + 6Na+ + 6e → 2Na3Sb, corresponding to twelve moles of sodium ions and electrons stored in one mole of Sb2S3.9,10 However, similar to the case of other sulfides, the serious volume change during the electrochemical reaction process would lead to poor reversibility and cycling performance. Moreover, because of a huge band gap energy (1.72 eV), Sb2S3 exhibits poor conductivity at room temperature (10−8 to 10−9 S cm−1).11 To address these issues, some methods have been applied that can be summarized as follows: (1) the design of a unique morphology or porous materials, such as bundle-like Sb2S3 (ref. 12) and flower-like Sb2S3,13 to alleviate the volume changes and (2) combining Sb2S3 with carbon materials or other conductive materials (graphite,9 graphene,14 polypyrrole,10 and carbon fiber15).

As is known, the Sb2S3 compound is generally prepared by chemical synthesis methods such as hydrothermal reaction,16 solvothermal reaction,17 and vacuum thermal evaporation.18 The abovementioned methods have several or fewer problems: complicated procedures, more by-products, low yield and others. Furthermore, the Sb element in reaction agents (SbCl3, Sb(NO3)3, and SbF3) that are the main components in the preparation of Sb2S3 is obtained from stibnite or other antimony minerals via different extraction techniques; the traditional and common extraction approaches of the mineral include electrolysis in an alkaline or strong acid solution, multiple volatilization, smelting and roasting reduction method, which cause high pollution, high time and energy consumption, and the generation of more hazardous waste. Therefore, stibnite or other antimony minerals are directly utilized as active materials in electrodes, which can effectively avoid the middle steps of Sb extraction as well as the synthesis of Sb2S3 that meet the environmentally friendly concept. Stibnite is a primary Sb2S3 mineral and belongs to the orthorhombic system (a0 = 11.20 Å, b0 = 11.28 Å, and c0 = 3.83 Å), which has been found in huge crystals and crystal clusters in many regions.19 Note that the natural pure mineral usually exhibits unfavorable electrochemical properties.20 Hence, it is necessary to improve the electrochemical sodium storage performances of the natural mineral with green manufacture methods.

In this study, the natural stibnite minerals that act as the main active materials have been directly applied for sodium storage. To improve the electrochemical performance of the natural stibnite ore, an effective and unsophisticated approach was adopted to prepare graphite/stibnite (G/Sb2S3) anode materials with excellent properties via the anchoring of the natural stibnite mineral on graphite under facile conditions. Furthermore, the G/Sb2S3 composites exhibit better electrochemical behaviors than the pure natural stibnite mineral owing to the introduction of graphite, which has a lamellar structure and high electric conductivity; this indicates the potentials of this mineral for large-scale energy storage applications; finally, this study is expected to promote the development of antimony sulfide materials that are eco-friendly and consume less energy and also offers a reference that natural minerals can be fully used as first-hand materials in energy storage.

2. Experimental

2.1 Preparation of active graphite and G/Sb2S3

All reagents were purchased and used without further purification. The procedures for the formation of active graphite were conducted as follows: (1) the commercial graphite was dispersed in mixed acid (HNO3[thin space (1/6-em)]:[thin space (1/6-em)]H2SO4 = 3[thin space (1/6-em)]:[thin space (1/6-em)]1, v/v) under magnetic stirring and then refluxed under 80 °C; (2) after 2 h, the active graphite was washed to become neutral and obtained. The G/Sb2S3 composites were prepared as follows: (1) 0.1 g active graphite was dispersed in 20 ml deionized water under ultrasonication for 4 h as the A solution; (2) 0.2 g natural stibnite ore (Sb2S3 ≥ 99%) was dispersed in 30 ml ethylene glycol under ultrasonication for 4 h as the B solution; (3) the A solution was added to the B solution, and then, the mixed solution was further stirred for 24 h; and (4) the mixed solution was transferred to a hydrothermal reactor at 150 °C for 12 h, and finally, the G/Sb2S3 composites were washed and obtained.

2.2 Material characterization

Thermogravimetric analysis (TGA, NETZSCH STA449F3), X-ray photoelectron spectroscopy (XPS a K-alpha 1063), X-ray diffraction (XRD, Bruker D8 diffractometer, Cu Kα radiation), transmission electron microscopy (TEM, JEM-2100F), scanning electron microscopy (SEM, FEI Quanta 200) and Raman spectroscopy (Renishaw inVia, UK, the wavelength of 0.1542 nm) were used to analyse the composites.

2.3 Electrochemical measurements

The electrode slurry was made up of 70 wt% G/Sb2S3 composites, 15 wt% carboxymethyl cellulose (CMC) and 15 wt% super P, which were dissolved in deionized water. Then, the even slurry was cast on a Cu foil followed by drying at 80 °C for 8 h. The electrolyte consists of 1 M NaClO4 dissolved in propylene carbonate (PC) with additional 5% fluoroethylene carbonate (FEC). The electrochemical properties were characterized by the CR2016-type half-cells with Celgard 2400 as the polypropylene separator, which were assembled in a glove box under an Ar atmosphere. Cyclic voltammetry (CV) was conducted at the scan rate of 0.1 mV s−1 in the voltage range from 0.01 to 2.5 V. Galvanostatic cycling and rate performances were tested at different current densities via an Arbin battery cycler (BT2000) in the voltage range from 0.01 to 2.5 V. Electrochemical impedance spectroscopy (EIS) was conducted in the frequency range from 0.01 Hz to 100 kHz using the CHI660E electrochemical workstation.

3. Results and discussion

To analyse the crystal structure, the G/Sb2S3 composites and stibnite mineral were investigated via X-ray diffraction (XRD). As illustrated in Fig. 1a, all the observed diffraction peaks were well matched to the orthorhombic phase of antimony sulfide (PDF# 42-1393, Pnma (62), a = 10.9590 Å, b = 2.8060 Å, and c = 10.9830 Å). These peaks were located at around 15.7°, 17.5°, 22.3°, 24.9°, 29.3°, 32.3°, 35.5° and 54.6°, which belonged to the (200), (120), (220), (130), (211), (221), (240) and (630) crystal planes of Sb2S3, respectively. Note that a sharp and intense peak of graphite at around 26.3° can be observed, which corresponds to the (002) crystal planes of graphite.21 Evidently, no other peaks were observed; this indicated high purity of the composites. Moreover, the peaks of the G/Sb2S3 composites are sharp and pointed, indicating that these composites have a good crystalline nature.22 As presented in Fig. 1b, thermogravimetric analysis (TGA) was conducted to compute the Sb2S3 content in the G/Sb2S3 composite under an air atmosphere from room temperature to 800 °C. With an increase in temperature, the carbon matrix was burned into CO2, and Sb2S3 was converted into Sb2O4.23 Finally, the content of Sb2S3 in the G/Sb2S3 composite was determined to be 66.68 wt%.
image file: c9ra02663k-f1.tif
Fig. 1 (a) XRD patterns of G/Sb2S3 and stibnite. (b) TGA curves of G/Sb2S3 and stibnite. (c) Raman spectra of G/Sb2S3 and stibnite. (d) Raman spectra of Sb–S.

Raman spectroscopy was conducted to investigate the variation of G/Sb2S3 composite and stibnite. As shown in Fig. 1c, the typical peaks of Sb2S3 were located at the range from 100 to 600 cm−1, and two obvious and intense peaks corresponding to the D-band and G-band of the graphite were observed. The peak at 1354 cm−1 was ascribed to the D-band, and a particular peak of the Csp3 hybrid orbital resulted from the disordered arrangement of carbon atoms or lattice defects;24 the other peak at 1581 cm−1 was attributed to the G-band, indicating an ordered lattice structure originating from the vibration of Csp2 in the plane.25 Generally, the disordered extent of the carbon materials could be expressed via the integrated intensity ratio ID/IG, which was 0.15 in the G/Sb2S3 composite, suggesting that the graphite still maintained a highly complete structure after the activation procedure. As depicted in Fig. 1d, the typical peaks of Sb2S3 are located at 122, 149, 187, 246, 309 and 446 cm−1, indicating the S–Sb stretching vibration and S–Sb–S bending vibration.26 Practically, the peaks at 122, 149 and 187 cm−1 are associated with the S–Sb–S bending vibration, and the shift at 246 cm−1 is related to the S–Sb stretching, indicating well-crystallinity of the proposed materials. The peak at 309 cm−1 was assigned to the symmetric vibration of the C3v symmetric pyramidal SbS3 unit.27 Specially, the inconspicuous peak at 446 cm−1 was attributed to the symmetric stretching of Sb–S–S–Sb.

To characterize the chemical composition and surface electronic states of G/Sb2S3, X-ray photoelectron spectroscopy (XPS) was conducted. As exhibited in Fig. 2a, these peaks of Sb2S3 were especially obvious from Sb (4d, 3d, 3p, 3s, Sb MNN) and S (2p, 2s), and all other peaks were weak and broad, which could be due to energy loss.28 In addition, it is obvious that many researchers have studied the Sb 3d spectroscopy of antimony compounds because of the higher intensity of Sb 3d than that of Sb 4d. As illustrated in Fig. 2b, the peaks of Sb 3d3/2 are located at 539.2 and 540.1 eV, whereas those of Sb 3d5/2 are located at 529.6 and 530.1 eV, indicating the existence of Sb3+.29 As shown in Fig. 2c, the peaks at 284.6, 285 and 286.1 eV are related to C[double bond, length as m-dash]C, C–C and O–C[double bond, length as m-dash]C, respectively, suggesting the existence of oxygen-containing functional groups that may suffer from partial oxidation during the activation step of graphite.30,31 The S 2p spectrum in Fig. 2d exhibits peaks at 161.3 and 162.5 eV, assigned to S 2p3/2 and S 2p1/2, respectively, which are confirmed to be a single doublet from the S–Sb bonds.32


image file: c9ra02663k-f2.tif
Fig. 2 (a) XPS survey of G/Sb2S3 and stibnite. The corresponding high-resolution spectra of Sb (b), S (c) and C (d).

The detailed morphology and crystal structure of the G/Sb2S3 composites and stibnite mineral were observed using a scanning electron microscope (SEM) and transmission electron microscope (TEM). As observed in Fig. 3a and b, the stibnite mineral has indistinctive morphology and uneven particle size. As observed from Fig. 3c–f, the small stibnite ore particles are uniformly decorated on the bulk graphite with the average dimension of around 10 μm, which can effectively enhance the conductivity of composites. As shown in the Fig. 3g and h, the lattice distances of 0.36 nm and 0.51 nm are assigned to the (130) plane and (120) plane of orthorhombic Sb2S3 crystals, respectively, which are consistent with the analysis of XRD.33,34 Moreover, the lattice rim of 0.34 nm corresponds to the (002) plane of graphite.35


image file: c9ra02663k-f3.tif
Fig. 3 (a and b) SEM image of stibnite. (c–f) SEM image of the G/Sb2S3 composites. (g and h) TEM image of the G/Sb2S3 composites. (i) HR-TEM image of the G/Sb2S3 composites.

Electrochemical properties of the G/Sb2S3 composites and stibnite mineral as SIBs anodes were evaluated by cyclic voltammetry in the potential range of 0.01–2.5 V. As shown in Fig. 4a, two current peaks at 0.78 V and 0.12 V were revealed in the initial cathodic scan, which were ascribed to the conversion reaction with sulfur atoms in composites (Sb2S3 + 6Na+ +6e → 2Sb + 3Na2Sb), alloying reaction of antimony with sodium (2Sb + 6Na+ + 6e → 2Na3Sb) and the side reaction to form the solid electrolyte interface (SEI) on the surface of the electrode, respectively.36


image file: c9ra02663k-f4.tif
Fig. 4 Cyclic voltammograms of initial three cycles of (a) G/Sb2S3 composites, (b) stibnite. (c) Galvanostatic discharge/charge curves of G/Sb2S3 composites. (d) Cycling performance and coulombic efficiencies of G/Sb2S3 and stibnite.

In the succeeding cathodic scans, the differences of CV curves could be explained by the formation of an SEI and other irreversible reactions in the initial cycle. Furthermore, the area of the initial scan was larger than that of the subsequent cycles, suggesting that its initial capacity was higher than that in the subsequent cycles.37 During the anodic scan, the peaks at 0.81 V and 1.61 V were respectively ascribed to the dealloying reaction (2Na3Sb → 2Sb + 6Na+ + 6e) and the formation of Sb2S3 (2Sb + 3Na2S → Sb2S3 + 6Na+ + 6e).38

The galvanostatic cycling test was conducted to investigate the electrochemical behaviors of the G/Sb2S3 composites at the current density of 0.1 A g−1 in the potential range of 0.01–2.5 V. As illustrated in Fig. 4c, in the first discharge profile, two smooth voltage plateaus at 1.18–0.85 V and 0.67–0.31 V corresponded to the reductive transformation and alloying reactions, respectively. In contrast, the voltage plateaus around at 0.63–1.16 V and 1.25–1.46 V were ascribed to the dealloying reactions and desodiation reactions in the charge profiles. Moreover, these plateau regions of discharge/charge agree well with the related CV curves.

The cycling performances of the G/Sb2S3 and stibnite mineral were studied at the current density of 0.1 A g−1 in the voltage range of 0.01–2.5 V. The G/Sb2S3 composites and stibnite mineral revealed a completely different electrochemical performance because of the introduction of graphite. As illustrated in Fig. 4d, the G/Sb2S3 composite delivered the initial charge/discharge capacity of 542.8/864 mA h g−1 with the coulombic efficiency (CE) of 62.76%, whereas the stibnite mineral exhibited the initial charge/discharge capacity of 617.8/1008.3 mA h g−1 with the lower CE of 61.27%. In addition, low initial coulombic efficiency is a common problem in conversion-alloying type materials.39 On the one hand, the formation of SEI originates from the decomposition of organic electrolytes at low voltages and the side reactions of the oxygen-containing functional groups on the surface of graphite with sodium ions, which can cause irreversible capacity.40 However, a stable SEI may also alleviate the irreversible reactions, which can improve coulombic efficiency in subsequent cycles evidently.41 Encouragingly, the G/Sb2S3 composites still exhibit the reversible capacity of 407 mA h g−1 with a 75.2% capacity retention, which are better than stibnite ore with 190.1 mA h g−1 and the capacity retention of 30.7% after 80 cycles. Evidently, the introduction of graphite could improve the capacity and reversibility of the stibnite mineral.

As shown in Fig. 5a, the rate performances of the G/Sb2S3 composites and stibnite mineral were further studied at different currents ranging from 0.1 A g−1 to 1 A g−1. The G/Sb2S3 composites delivered the average reversible capacities of 642.3, 507.6, 392.1 and 264.9 mA h g−1 at the current densities of 0.1, 0.3, 0.5 and 1 A g−1, respectively. A similar capacity loss could be observed in stibnite mineral. Furthermore, the average reversible capacity of the G/Sb2S3 composites could recover to 595 mA h g−1 when the current density was back to 0.1 A g−1 after 20 cycles. The cycling stability is key indicator to evaluate anode materials for application. Herein, the G/Sb2S3 composites were further studied at the current density of 0.2 A g−1 following the rate evaluation. After 75 cycles, the reversible capacity was 422 mA h g−1 with the capacity retention of 82.9%. However, the stibnite mineral delivered poorer cycling performance. According to these differences, graphites in the composites might have a positive influence on enhancing the electrochemical performance of the stibnite mineral. Electrochemical impedance spectroscopy (EIS) was conducted in the frequency range from 0.01 to 100 kHz at room temperature. The typical Nyquist plot consists of a depressed semicircle in the medium-high frequency region and a sloping line in the low frequency region, corresponding to the formation of a passivation layer and impedance between the electrolyte and active materials.42 Moreover, the charge transfer impedance (Rct) as the main part of the whole kinetic impedance of the battery was illustrated by the semicircle at a medium frequency, which could be computed via utilizing the diameter of the semicircle.40 The Warburg impedance was evaluated to the diffusion process of sodium ions in anode materials, which is depicted in the sloping line at the low frequency.40 As illustrated in Fig. 5b, the G/Sb2S3 composites delivered lower computed Rct (547 Ω) than that of stibnite mineral electrode (785 Ω), indicating the decreased charge transfer of G/Sb2S3 composites at the interface of electrode and electrolyte. Furthermore, the slope of G/Sb2S3 was more vertical than that of stibnite mineral at low frequency, suggesting better diffusion of sodium ions in the electrode.42 From the Fig. 5c, the initial impedance of G/Sb2S3 composites were higher than the cycled electrode, suggesting an activation process and formation of stable SEI on the surface of the electrode during the insertion/desertion process. The improved diffusivity of sodium ions and conductivity of G/Sb2S3 composites benefited from the introduction of graphite, which was initiated to enhance the kinetics of the electrochemical reaction.


image file: c9ra02663k-f5.tif
Fig. 5 (a) Rate performance of the Sb2S3 electrode. (b) Nyquist plots of G/Sb2S3 and stibnite at the initial state. (c) Nyquist plots of G/Sb2S3 at different states.

4. Conclusion

In summary, the G/Sb2S3 composites were successfully fabricated using the natural stibnite mineral and graphite via a novel and facile strategy, and their sodium storage performance was also investigated. Compared with the pure stibnite mineral, the G/Sb2S3 composite electrode exhibited excellent cycling rate properties as the SIB anodes. The improved performance was most possibly ascribed to the introduction of graphite that might have effectively enhanced the conductivity of the stibnite mineral and accommodated the volume changes of Sb2S3. This study demonstrates that natural stibnite minerals as first-hand materials can be applied in SIBs and is expected to provide environmental ideas that natural minerals after simple modifications can be directly applied in the energy storage domain.

Conflicts of interest

There are no conflicts to declare.

Acknowledgements

This work was financially supported by the Young Elite Scientists Sponsorship Program by CAST (2017QNRC001), National Natural Science Foundation of China (51904342, 51622406, 21673298), Hunan Provincial Natural Science Foundation of China (2018JJ3633), National Postdoctoral Program for Innovative Talents (BX00192), and National Key Research and Development Program of China (2017YFB0102000, 2018YFB0104200).

References

  1. S. Dong, C. Li, X. Ge, Z. Li, X. Miao and L. Yin, ZnS-Sb2S3@C Core-Double Shell Polyhedron Structure Derived from Metal-Organic Framework as Anodes for High Performance Sodium Ion Batteries, ACS Nano, 2017, 11, 6474–6482 CrossRef CAS PubMed.
  2. E. M. Lotfabad, J. Ding, K. Cui, A. Kohandehghan, W. P. Kalisvaart, M. Hazelton and D. Mitlin, High-Density Sodium and Lithium Ion Battery Anodes from Banana Peels, ACS Nano, 2014, 8, 7115–7129 CrossRef CAS PubMed.
  3. J. Song, P. Yan, L. Luo, X. Qi, X. Rong, J. Zheng, B. Xiao, S. Feng, C. Wang, Y.-S. Hu, Y. Lin, V. L. Sprenkle and X. Li, Yolk-shell structured Sb@C anodes for high energy Na-ion batteries, Nano Energy, 2017, 40, 504–511 CrossRef CAS.
  4. W. Yang, H. Wang, T. Liu and L. Gao, A Bi2S3@CNT nanocomposite as anode material for sodium ion batteries, Mater. Lett., 2016, 167, 102–105 CrossRef CAS.
  5. H. Hou, G. Zou, P. Ge, G. Zhao, W. Wei, X. Ji and L. Huang, Synergistic effect of cross-linked carbon nanosheet frameworks and Sb on the enhancement of sodium storage performances, New J. Chem., 2017, 41, 13724–13731 RSC.
  6. C. Zhang, X. Wang, Q. Liang, X. Liu, Q. Weng, J. Liu, Y. Yang, Z. Dai and K. Ding, Amorphous Phosphorus/Nitrogen-Doped Graphene Paper for Ultrastable Sodium-Ion Batteries, Nano Lett., 2016, 16, 2054–2060 CrossRef CAS PubMed.
  7. Z. Liu, X.-Y. Yu, X. W. Lou and U. Paik, Sb@C coaxial nanotubes as a superior long-life and high-rate anode for sodium ion batteries, Energy Environ. Sci., 2016, 9, 2314–2318 RSC.
  8. G. Zhao, G. Zou, X. Qiu, S. Li, T. Guo, H. Hou and X. Ji, Rose-like N-doped Porous Carbon for Advanced Sodium Storage, Electrochim. Acta, 2017, 240, 24–30 CrossRef CAS.
  9. Y. Zhao and A. Manthiram, Amorphous Sb2S3 embedded in graphite: a high-rate, long-life anode material for sodium-ion batteries, Chem. Commun., 2015, 51, 13205–13208 RSC.
  10. T. Zheng, G. Li, L. Zhao and Y. Shen, Flowerlike Sb2S3/PPy Microspheres Used as Anode Material for High-Performance Sodium-Ion Batteries, Eur. J. Inorg. Chem., 2018, 2018, 1224–1228 CrossRef CAS.
  11. M. Kriisa, M. Krunks, I. Oja Acik, E. Kärber and V. Mikli, The effect of tartaric acid in the deposition of Sb2S3 films by chemical spray pyrolysis, Mater. Sci. Semicond. Process., 2015, 40, 867–872 CrossRef CAS.
  12. Z. Yi, Q. Han, Y. Cheng, Y. Wu and L. Wang, Facile synthesis of symmetric bundle-like Sb2S3 micron-structures and their application in lithium-ion battery anodes, Chem. Commun., 2016, 52, 7691–7694 RSC.
  13. Y. Zhu, P. Nie, L. Shen, S. Dong, Q. Sheng, H. Li, H. Luo and X. Zhang, High rate capability and superior cycle stability of a flower-like Sb2S3 anode for high-capacity sodium ion batteries, Nanoscale, 2015, 7, 3309–3315 RSC.
  14. J. Zhou, B. Yan, J. Yang, Y. Yang, W. Zhou, H. Lan, H. Wang and L. Guo, A densely packed Sb2O3 nanosheet-graphene aerogel toward advanced sodium-ion batteries, Nanoscale, 2018, 10, 9108–9114 RSC.
  15. S. Liu, Z. Cai, J. Zhou, M. Zhu, A. Pan and S. Liang, High-performance sodium-ion batteries and flexible sodium-ion capacitors based on Sb2X3 (X = O, S)/carbon fiber cloth, J. Mater. Chem. A, 2017, 5, 9169–9176 RSC.
  16. C. Yan, G. Chen, R. Jin, X. Zou, H. Xu and C. Lv, Well-defined Sb2S3 nanostructures: citric acid-assisted synthesis, electrochemical hydrogen storage properties, Cryst. Res. Technol., 2013, 48, 566–573 CrossRef CAS.
  17. N. Maiti, S. H. Im, Y. H. Lee and S. I. Seok, Urchinlike nanostructure of single-crystalline nanorods of Sb2S3 formed at mild reaction condition, ACS Appl. Mater. Interfaces, 2012, 4, 4787–4791 CrossRef CAS PubMed.
  18. K. Zhou, M. Hu, Y.-b. He, L. Yang, C. Han, R. Lv, F. Kang and B. Li, Transition metal assisted synthesis of tunable pore structure carbon with high performance as sodium/lithium ion battery anode, Carbon, 2018, 129, 667–673 CrossRef CAS.
  19. C. G. Anderson, The metallurgy of antimony, Chem. Erde, 2012, 72, 3–8 CrossRef CAS.
  20. S. Li, H. Tang, P. Ge, F. Jiang, J. Zhou, C. Zhang, H. Hou, W. Sun and X. Ji, Electrochemical Investigation of Natural Ore Molybdenite (MoS2) as a First-Hand Anode for Lithium Storages, ACS Appl. Mater. Interfaces, 2018, 10, 6378–6389 CrossRef CAS PubMed.
  21. H. Liu, J. Huang, X. Li, J. Liu and Y. Zhang, SnO2 nanorods grown on graphite as a high-capacity anode material for lithium ion batteries, Ceram. Int., 2012, 38, 5145–5149 CrossRef CAS.
  22. J. Kong, H. Wei, D. Xia and P. Yu, High-performance Sb2S3/Sb anode materials for Li-ion batteries, Mater. Lett., 2016, 179, 114–117 CrossRef CAS.
  23. A. S. Hameed, M. V. Reddy, J. L. T. Chen, B. V. R. Chowdari and J. J. Vittal, RGO/Stibnite Nanocomposite as a Dual Anode for Lithium and Sodium Ion Batteries, ACS Sustainable Chem. Eng., 2016, 4, 2479–2486 CrossRef CAS.
  24. G. Zou, C. Wang, H. Hou, C. Wang, X. Qiu and X. Ji, Controllable Interlayer Spacing of Sulfur-Doped Graphitic Carbon Nanosheets for Fast Sodium-Ion Batteries, Small, 2017, 13, 1700762 CrossRef PubMed.
  25. G. Wang, X. Xiong, Z. Lin, C. Yang, Z. Lin and M. Liu, Sb/C composite as a high-performance anode for sodium ion batteries, Electrochim. Acta, 2017, 242, 159–164 CrossRef CAS.
  26. J. Ibáñez, J. A. Sans, C. Popescu, J. López-Vidrier, J. J. Elvira-Betanzos, V. P. Cuenca-Gotor, O. Gomis, F. J. Manjón, P. Rodríguez-Hernández and A. Muñoz, Structural, Vibrational, and Electronic Study of Sb2S3 at High Pressure, J. Phys. Chem. C, 2016, 120, 10547–10558 CrossRef.
  27. Q. Ru, X. Chen, B. Wang, Q. Guo, Z. Wang, X. Hou and S. Hu, Biological carbon skeleton of lotus-pollen surrounded by rod-like Sb2S3 as anode material in lithium ion battery, Mater. Lett., 2017, 198, 57–60 CrossRef CAS.
  28. V. P. Zakaznova-Herzog, S. L. Harmer, H. W. Nesbitt, G. M. Bancroft, R. Flemming and A. R. Pratt, High resolution XPS study of the large-band-gap semiconductor stibnite (Sb2S3): structural contributions and surface reconstruction, Surf. Sci., 2006, 600, 348–356 CrossRef CAS.
  29. S. Wang, S. Liu, X. Li, C. Li, R. Zang, Z. Man, Y. Wu, P. Li and G. Wang, SnS2-Sb2S3 Heterostructures Anchored on Reduced Graphene Oxide Nanosheets with Superior Rate Capability for Sodium-Ion Batteries, Chem. Eur J., 2018, 24, 3873–3881 CrossRef CAS PubMed.
  30. Y. Wu, L.-Y. Wang, Y.-F. Li, Z.-Y. Zhao, L.-W. Yin, H. Li and Y.-J. Bai, KCl-Modified Graphite as High Performance Anode Material for Lithium-Ion Batteries with Excellent Rate Performance, J. Phys. Chem. C, 2017, 121, 13052–13058 CrossRef CAS.
  31. L. Chen, R. Lin and C. Yan, Nitrogen-doped double-layer graphite supported CuCo2S4 electrode for high-performance asymmetric supercapacitors, Mater. Lett., 2019, 235, 6–10 CrossRef CAS.
  32. K. Xiao, Q. Z. Xu, K. H. Ye, Z. Q. Liu, L. M. Fu, N. Li, Y. B. Chen and Y. Z. Su, Facile Hydrothermal Synthesis of Sb2S3 Nanorods and Their Magnetic and Electrochemical Properties, ECS Solid State Lett., 2013, 2, P51–P54 CrossRef CAS.
  33. J.-H. Choi, C.-W. Ha, H.-Y. Choi, H.-C. Shin, C.-M. Park, Y.-N. Jo and S.-M. Lee, Sb2S3 embedded in amorphous P/C composite matrix as high-performance anode material for sodium ion batteries, Electrochim. Acta, 2016, 210, 588–595 CrossRef CAS.
  34. X. Guo, X. Xie, S. Choi, Y. Zhao, H. Liu, C. Wang, S. Chang and G. Wang, Sb2O3/MXene(Ti3C2Tx) hybrid anode materials with enhanced performance for sodium-ion batteries, J. Mater. Chem. A, 2017, 5, 12445–12452 RSC.
  35. L. Wang, J. Yang, J. Li, T. Chen, S. Chen, Z. Wu, J. Qiu, B. Wang, P. Gao, X. Niu and H. Li, Graphite as a potassium ion battery anode in carbonate-based electrolyte and ether-based electrolyte, J. Power Sources, 2019, 409, 24–30 CrossRef CAS.
  36. P. Ge, H. Hou, X. Ji, Z. Huang, S. Li and L. Huang, Enhanced stability of sodium storage exhibited by carbon coated Sb2S3 hollow spheres, Mater. Chem. Phys., 2018, 203, 185–192 CrossRef CAS.
  37. J. Pan, Z. Zuo, J. Deng, Q. Yao, Z. Wang and H. Zhou, Sb2S3 single crystal nanowires with comparable electrochemical properties as an anode for sodium ion batteries, Surf. Interfaces, 2018, 10, 170–175 CrossRef CAS.
  38. H. Hou, M. Jing, Z. Huang, Y. Yang, Y. Zhang, J. Chen, Z. Wu and X. Ji, One-Dimensional Rod-Like Sb2S3-Based Anode for High-Performance Sodium-Ion Batteries, ACS Appl. Mater. Interfaces, 2015, 7, 19362–19369 CrossRef CAS PubMed.
  39. S. Wang, S. Yuan, Y.-B. Yin, Y.-H. Zhu, X.-B. Zhang and J.-M. Yan, Green and Facile Fabrication of MWNTs@Sb2S3@PPy Coaxial Nanocables for High-Performance Na-Ion Batteries, Part. Part. Syst. Charact., 2016, 33, 493–499 CrossRef CAS.
  40. Y. Dong, S. Yang, Z. Zhang, J. M. Lee and J. A. Zapien, Enhanced electrochemical performance of lithium ion batteries using Sb2S3 nanorods wrapped in graphene nanosheets as anode materials, Nanoscale, 2018, 10, 3159–3165 RSC.
  41. M. Hu, Y. Jiang, W. Sun, H. Wang, C. Jin and M. Yan, Reversible conversion-alloying of Sb2O3 as a high-capacity, high-rate, and durable anode for sodium ion batteries, ACS Appl. Mater. Interfaces, 2014, 6, 19449–19455 CrossRef CAS PubMed.
  42. Z. Zhang, J. Zhao, M. Xu, H. Wang, Y. Gong and J. Xu, Facile synthesis of Sb2S3/MoS2 heterostructure as anode material for sodium-ion batteries, Nanotechnology, 2018, 29, 335401 CrossRef PubMed.

This journal is © The Royal Society of Chemistry 2019
Click here to see how this site uses Cookies. View our privacy policy here.