Lenka Procházková*ab,
Vojtěch Vaněčeka,
Václav Čubaa,
Radek Pjatkanc,
Rosana Martinez-Turtosd,
Ivo Jakubece,
Maksym Buryib,
Sergey Omelkovf,
Etiennette Auffrayg,
Paul Lecoqg,
Eva Mihókováab and
Martin Niklb
aCzech Technical University in Prague, Faculty of Nuclear Sciences and Physical Engineering, Břehová 7, 115 19 Czech Republic. E-mail: lenka.prochazkova@fjfi.cvut.cz
bInstitute of Physics of the AS CR, v.v.i, Cukrovarnická 10, Prague 6, Czech Republic
cNUVIA a.s., Trojanova street 117, 278 01 Kralupy nad Vltavou, Czech Reublic
dUniversità degli Studi di Milano Bicocca, Piazza della Scienza 3, 20126, Milano, Italy
eInstitute of Inorganic Chemistry of the Czech Academy of Sciences, Řež 250 68, Husinec-Řež 1001, Czech Republic
fInstitute of Physics, University of Tartu, W. Ostwaldi 1, 50411 Tartu, Estonia
gCERN, 1211 Geneva 23, Switzerland
First published on 17th September 2019
Heat treatment is needed to increase the luminescence intensity of ZnO:Ga particles, but it comes at the cost of higher particle agglomeration. Higher agglomeration results in low transparency of scintillating powder when embedded in a matrix and constitutes one of the biggest disadvantages, besides low light yield and low stopping power, of ZnO:Ga powder. Limiting ZnO:Ga particle size is therefore a key step in order to prepare highly luminescent and transparent composites with prospects for optical applications. In this work, SiO2 coating was successfully used to improve luminescence intensity or limitation of crystallite size growth during further annealing. Furthermore, ZnO:Ga and ZnO:Ga-SiO2 core–shells were embedded in a polystyrene matrix.
It is known that the luminescence intensity in nanocrystals of direct gap semicondcutors can be strongly reduced due to the surface defects (vacancies, non-saturated bonds or adsorbed species) acting as charge carrier traps and nonradiative recombination centers and various strategies have been adopted to suppress them.9–11 Their negative effect can be healed by frequently used surface passivation12,13 effectively implemented as a shell formed around the active core. Resulting core–shell systems are currently investigated and exploited in a number of applications. Core–shell quantum dots (QDs) based on CdSe core and a variety of shells are already applied in light emitting diodes for monitors and TV screens14–18 or photovoltaics.19,20 Together with Cd-free QDs they are also studied for biomedical applications.12,21
Shell layer can serve many purposes depending on the nature of the material and its desired characteristics. The shell can protect the core material from environment, improve its poor mechanical properties or alter its optical properties.22 Recently, various methods have been studied for passivation or modification of the nanoparticle (NP) surface, depending on the target application.23,24 The surface coverage by either organic polymers or inorganic (amorphous, semi-crystalline or crystalline) layers was implemented. Properly chosen and applied outer layer in core–shell materials can limit the particle agglomeration which occurs during annealing at higher temperatures25 and/or improve their optical properties, such as the light yield or decay time.26 One can grow an inorganic solid shell on the core via a sol–gel route, cover the core by organic ligands or grow a polymer shell by a polymerization process to make the core biocompatible.27
Sol–gel route to synthesize ZnO@SiO2 core–shell systems has already been reported.28 Alternatively, hydrothermally-prepared ZnO cores were coated by SiO2 and then selectively etched by the aqueous solution of HCl.29 Scanning electron microscope (SEM) images and energy-dispersive spectra (EDS) clearly showed hollow SiO2 shells and confirmed successful synthesis of the ZnO@SiO2 core–shell composites. A deposition of SiO2 layer on ZnO nanowires via reactive sputtering to passivate native point defects was used.12 The passivation of oxygen vacancies resulted in strong suppression of the visible emission and the effect of annealing at higher temperatures (700-900 °C) was also studied.
The coating of ZnO nanorods by Al2O3 and hydrogen plasma treatment were investigated to passivate the surface states associated with the deep-level emission in the green spectral area.13 Coating by MgO was tested,30 however the overall intensity of emission decreased with increasing MgO layer thickness above 15 nm. Selected optoelectronic properties may be improved by the adsorption of organic layer on the ZnO nanoparticles.31 Thus, the wavelength selectivity and UV absorbance was significantly improved by the adsorption of DMF on the ZnO NPs surface. To stabilize colloidal particles, organic surfactants or polymers may be used, e.g. polymer thin shell has been synthesized on the ZnO nanoparticle surface from pre-existing inherent free radicals.32
Recently, high attention has been devoted to the preparation of thin films on substrates or composite materials where scintillating nanopowders and nanoparticles are immobilized in the optically transparent matrices. There are several works reporting on the luminescent properties of ZnO embedded into more or less transparent organic materials and a wide range of polymers was investigated.33–35 However, polystyrene (PS) matrix currently seems to be the most promising due to its convenient luminescence properties.2,36 Specifically, the PS matrix itself is an efficient scintillator and moreover, an energy transfer from the matrix to the scintillating ZnO crystals is possible.36 ZnO:Ga-polystyrene composites (ZnO:Ga-PS) were prepared and already reported in Burešová et al., 2016,36 where 10 wt% filling with powder was used; characterization of the composite showed that low transparency does not allow sufficient transmission of emitted light.
For an actual design of optical devices based on nanoparticles embedded in host matrices, two key problems need to be solved; increasing the intensity of radioluminescence to sufficient level comparable with single crystals or optical ceramics and limiting the growth of nanoparticles, so that they can be embedded in sufficient amount without decreasing the optical transparency of the matrix.
In this work, we study the surface defect passivation and limiting growth of luminescent ZnO:Ga particles by SiO2 coating and embedding in polystyrene (PS) matrix together with the effect of these procedures on luminescence properties. We also compare ZnO:Ga-PS with core–shell ZnO:Ga-SiO2-PS at various levels of filling.
X-ray powder diffraction (XRPD) was used for structural and phase analysis. XRPD was performed using Rigaku MiniFlex 600 (Ni-filtered Cu-Kα 1,2 radiation) equipped with NaI:Tl scintillation detector and diffractograms were compared to the relevant records in the ICDD PDF-2 database (version 2013). Determination of the specific surface area of the samples by single point BET method was carried out on Monosorb MS-22 (Quantachrome Instruments) using the mixture containing 30% of nitrogen and 70% of helium as a carrier gas. Further characterization was performed using scanning electron microscopy (SEM, Philips XL30CP) high resolution transmission electron microscopy (HRTEM, JEOL 3010), and selected area electron diffraction (SAED). Luminescence properties were evaluated by measuring photoluminescence (PL) steady-state and time-resolved spectra as well as the radioluminescence (RL) spectra using the custom-made spectrofluorometer 5000 M, Horiba JobinYvon. X-ray tube (RL spectra) and nanoLED 339 nm (PL decays) were used as the excitation sources. Detection part of the set-up consisted of single grating monochromator and photon counting detector TBX-04. Time-correlated single photon counting technique was utilized to measure subnanosecond PL decays and measured spectra were corrected for the spectral dependence of detection sensitivity. PL decays were determined by convolution procedure (SpectraSolve software package, Ames Photonics). RL decay measurements were performed in time correlated single photon counting using a pulsed tungsten X-ray tube and a fast hybrid PMT from Becker & Hickl with a FWHM of around 55 ps. Photons are integrated over the entire spectral range from 220–800 nm with no further discrimination. The impulse response function of the whole setup (laser + X-ray tube + photodetector + electronic readout) has been obtained by means of intraband luminescence present in Li2MoO4 crystals with a final FWHM of around 130 ps. For more details, please refer to ref. 37.
(1) |
The superstoichiometric amount of ammonium hydroxide was added dropwise and the suspension was stirred for 5 hours to ensure the complete hydrolysis of TEOS. Product was washed by ethanol and water, separated and dried.
In particle agglomeration study, the SiO2 coated ZnO:Ga nanopowder processed according to (i) was subsequently annealed at 400 °C, 600 °C and 1000 °C and the effect on the crystallinity, particle size and phase purity was investigated. RL spectra were measured for ZnO:Ga-SiO2 core–shells where annealed powder was used as a core material.
Fig. 2 HRTEM images of ZnO:Ga-SiO2 without further heat treatment (left) and after treatment at 1000 °C (right). |
The morphology of ZnO:Ga-SiO2 core–shells was investigated using SEM, HRTEM and EDX. SEM images with EDX show spherical particles of varying size and lower Zn concentration (Fig. 4). TEM images prove that hexagonal zinc oxide crystals occur in the centre of spherical formations in many cases (Fig. 5), but also pure amorphous SiO2 particles are formed. This unwanted effect is likely to be suppressed by the optimization of TEOS concentration and kinetics of the SiO2 layer growth.
Fig. 4 SEM images of ZnO:Ga-SiO2 particles with EDX element analysis. Turquoise colour represents zinc, yellow colour represents silicon. |
RL spectra of ZnO:Ga-SiO2 core–shells feature significantly increased intensity of the emission with maxima at 390 nm in comparison with pure ZnO:Ga particles (Fig. 6). We assume, that homogeneous SiO2 shell on the surface of ZnO:Ga scintillating core heals the surface defects, thus contributing to the increase of RL intensity. Improving luminescence intensity may be explained by the healing of the surface defects and passivation of surface states, as mentioned in ref. 31 and 32. In Fu et al., 201138 the authors propose that the reduction in trap density within the band gap causing preferred radiative recombination near the band edge is due to the passivation of dangling bonds and O2− ions on the surface. Moreover, Sombrio et al.12 suggest the improving of ZnO/SiO2 interface due to the Zn–O–Si bond formation above certain temperature as a possible explanation.
Fig. 8 RL spectra of ZnO:Ga-PS (1 wt%) and ZnO:Ga-SiO2-PS (1 wt%) composites (A) and composites with 5 wt% and 10 wt% filling (B). |
A series of photoluminescence decays as well as spectral-time resolved measurements using X-ray excitation source were performed. We expect that PS matrix is primarily excited under 281 nm, while ZnO:Ga particles are directly excited under 339 nm. Photoluminescence decays are shown in Fig. 9A and B. Minor slow component is noticeable under both 281 and 339 excitation wavelengths. In the case of the excitation of PS matrix, slow component (13.6 ns) may origin in the emission of PS itself. Direct excitation of ZnO:Ga particles features slow component about 4 ns, probably caused by capture of exciton on the interface of ZnO:Ga particles and PS matrix. Spectrally integrated data obtained by pulsed X-ray excitation for ZnO:Ga-PS and ZnO:Ga-SiO2-PS are shown in Fig. 10A and B. It is obvious that silica layer does not negatively affect timing performance and extremely short decay with practically zero rise time preserved. The decays do not show any presence of polystyrene host emission as already reported in ref. 2 and 36. The absence of PS slower emission in X-ray decays may be explained by transfer of energy absorbed by PS to ZnO particles. Values of several hundreds of picoseconds in PL and X-ray excited decays of fast excitonic ZnO or ZnO:Ga emission were also reported in literature. X-ray excited luminescence decays at RT of ZnO:Ga powders showed two components – 320 and 820 ps in ref. 42, 800 ps in ref. 7, ZnO nanowires treated through hydrogen plasma demonstrated faster decays from 300 to 140 ps at 10 K,43 PL decay time of free exciton in ZnO single crystal of 400 ps was observed at RT in ref. 44 and the value of about 1 ns is reported for ZnO:Ga ceramics.45
Fig. 9 PL decays of ZnO:Ga-PS (5 wt%) under 281 nm (A) and 339 nm (B) excitation and two-exponential fits. |
Fig. 10 Comparison of ZnO:Ga-PS (10 wt%) and ZnO:Ga-SiO2-PS (10 wt%) RL decays (A) and single-exponential fit for ZnO:Ga-SiO2-PS (10 wt%) sample (B). |
Covering ZnO:Ga scintillating particles by amorphous SiO2 layer via sol–gel process significantly improves the luminescence intensity due to the passivation of the particle surface defects.
Composites prepared by embedding ZnO:Ga-based particles in polystyrene with sufficient powder filling (∼10 wt%) show only strong UV emission from ZnO:Ga particles, but the low transparency limits their practical use. Composites with very low filling (1 wt%) exhibit also the emission from the PS matrix, while the 5 wt% filling is already sufficient to ensure an effective transfer of absorbed energy from the matrix to ZnO:Ga particles. Extremely short PL and RL decays between 200–700 ps with practically zero rise time were preserved. Slow component associated with PS is present only in the case of 1 wt% filling.
Presented results show methods for particle size limitation and surface passivation via silica covering and embedding in polymer matrix. These steps play a key role in the further development of scintillating nanomaterials for detectors. However, microstructural study of composite core–shell scintillators is an ongoing task.
Despite some disadvantages, synthesized ZnO:Ga-based scintillators show a strong promise for applications in future generation of detectors as well as photo/radiotherapy.39–41 ZnO:Ga-PS composites with appropriate composition have a high potential for use in fast-timing applications. Nevertheless, some improvements are needed. Even though annealing temperatures of the ZnO:Ga core are rather high, in possible future applications, annealing of large amounts of the material may reduce the cost. Despite that, lowering the annealing temperature is a high priority in future research, since it would also limit the particle agglomeration.
The study was carried out in the frame of Crystal Clear collaboration and received support from ERC grant no. 338953 TICAL, the EC H2020 project no. 690599 ASCIMAT and COST Action TD1401 (FAST).
This journal is © The Royal Society of Chemistry 2019 |