Haiyan Liua,
Mei Hana,
Jinzong Zuoa,
Xuexiang Denga,
Wenxue Lua,
Yongguo Wua,
Huaihe Song*b,
Chunli Zhoub and
Shengfu Jib
aNational Engineering Center of Coal Water Slurry Gasification and Coal Chemical, Yankuang Group, Tengzhou, Shandong 277527, P. R. China
bState Key Laboratory of Chemical Resource Engineering, Beijing University of Chemical Technology, Beijing, 100029, P. R. China. E-mail: songhh@mail.buct.edu.cn; Fax: +86-010-64434916; Tel: +86-010-64434916
First published on 21st May 2019
In this work, novel heteroatom-doped hollow carbon spheres (HHCSs) were prepared via the carbonization of polyaniline hollow spheres (PHSs), which were synthesized by one-pot polymerization. It was found that the carbonized PHSs at 700 °C exhibit high specific capacitance of 241 F g−1 at a current density of 0.5 A g−1 and excellent rate capability. The excellent electrochemical performance can be attributed to the heteroatom-doping and hollow carbon nanostructure of the HHCSs electrodes. Heteroatom groups in the HHCSs not only improve the wettability of the carbon surface, but also enhance the capacitance by addition of a pseudocapacitive redox process. Their unique structure provides a large specific surface area along with reduced diffusion lengths for both mass and charge transport.
Various types of carbon materials meeting the mechanism of the EDLCs have been used as electrode materials, such as activated carbons,4,5 carbon nanotubes,6 graphene,7 carbon aerogels8 and mesoporous carbons.9 Carbon-based electrode materials can offer lower specific capacitance and energy density in supercapacitor compared with most pseudocapacitor electrode materials such as metal oxides and conductive polymers. Doping carbonaceous materials with heteroatoms can couple the pseudocapacitance to the EDLCs while maintaining the excellent intrinsic characteristics of carbonaceous materials at the same time. Recently, many attempts have been devoted to the preparation of heteroatom-doped carbon-based materials.10–15 For example, heteroatom-doped carbonaceous materials have been obtained from gelatin,16 leaves,17 animal bones,18 banana fibers,19 rice husk,20 catkins21 and so on.
In addition to heteroatoms doping, an appropriate microstructure can improve the electrochemical performance of carbonaceous materials by providing high electrochemically accessible surface area.22 Hollow spheres are promising microstructure due to their high surface-to-volume ratios and reduced transport lengths for both mass and charge transport.23–27 Dong et al. reported a surfactant-assisted template method for synthesis of hollow carbon nanospheres by using polydopamine (PDA) as carbon source and ZnO as template.26 Nitrogen-containing carbon microspheres with hollow core exhibit the specific capacitance of 306 F g−1 at a current density of 0.1 A g−1 in 2 M H2SO4.27 Polyaniline (PANI) is considered as the most potential precursor because of its facile synthesis, environmental stability and high N/C ratio (0.167). PANI with various shapes has been produced28–32 by controlling the synthesis conditions. Through high temperature heat treatment in an inert gas atmosphere, carbon nanostructures with special morphologies are easily prepared from the PANI nanostructures by maintaining the original shapes of PANIs.14,15 A kind of nitrogen-doped hollow carbon spheres was synthesized by the use of sulfonated polystyrene spheres as a hard template.22 The hard template method is common but complicated since the template must be removed and the structure of product may be destroyed. Therefore, it is necessary to develop a facile, cost-effective strategy for synthesizing heteroatom-doped hollow carbon spheres (HHCSs).
Herein, we report a method to prepare HHCSs via carbonization of hollow PANI spheres (HPSs). During the high temperature treatment, condensation and polymerization result in amorphous carbon with microporous and heteroatom-doped structure. The obtained HHPSs show an excellent performance and rate capability as the electrode materials for supercapacitors. The excellent electrochemical performance is attributed to the heteroatom-doping and hollow carbon nanostructure of the HHCSs electrodes.
Fig. 2 SEM image of HPSs (a), TEM image of HPSs (b); SEM images of HHCSs-600 (c), HHCSs-700 (d) and HHCSs-800 (e); TEM image of HHCSs-700 (f). |
In order to get HHCSs, PHSs were heated in N2 gas atmosphere at different temperatures from 600 to 800 °C. During the high temperature treatment, condensation and polymerization take place with the escape of hydrogen and nitrogen atoms, remaining the carbon skeleton. With increasing temperature, the non-carbon atoms lost more, and the carbon skeleton would gradually shrink. The shape of HHCSs-600 and HHCSs-700 generally maintains well after heat treatment (Fig. 2c and d). As shown in Fig. 2e, the shape of HHCSs-800 seriously shrinks. The spheres collapse and connect together. From Fig. 2f, the diameter of the HHCSs-700 cavities and the thickness of the shells are about 400 nm and 80 nm, respectively. A highly developed microporous structure can form in HHCSs shell due to the pyrolysis and carbonization of the HPS. This unique porous hollow structure can provide a large specific surface area along with reduced diffusion lengths for both mass and charge transport.
Fig. 3 shows the XRD patterns of three samples. The XRD patterns of HHCSs exhibit one broad diffraction peak around 22°, which corresponds to the (002) facet of hexagonal graphitic carbon.34–36 By increasing the carbonization temperature from 600 to 800 °C, the intensity of the peak slightly increased, suggesting the elevated degree of graphitization.
X-ray photoelectron spectroscopy (XPS) was employed to further analyze the nature and amount of functional groups of the HHCSs. The chemical state of nitrogen atoms in carbonized samples is assigned to five types according to previous reports:37,38 398.4 eV (pyridinic nitrogen N-6), 400 eV (pyrrolic nitrogen N-5), 401 eV (quaternary nitrogen N-Q) and 402.6 eV (pyridine-N-oxide or ammonia), and 405.5 eV (chemisorbed nitrogen oxides N-X). Some previous studies indicated that nitrogen located at the edges of graphene layers, for example, N-6 and N-5, could represent the pseudocapacitance effect.16,39,40 N-6 enhances the capacitance owing to their positive charge, which allows fast electron transfer.5,41
Table 1 shows that the residual nitrogen content in the HHCSs is very high compared with those of other nitrogen-doped carbon materials.33,34,42,43 It was found that the obtained materials have oxygen-containing functional groups as well as nitrogen functional groups, which are advantageous for capacitance as they can considerably contribute to an additional pseudo-capacitance.44,45 Especially, oxygen functional groups can improve the wettability between electrode materials and electrolytes, depending on their hydrophilic nature.46,47 The binding energies around 531.5 eV, 532.6 eV, and 533.7 eV represent CO quinone type groups (O-1), C–OH phenol groups and/or C–O–C ether groups (O-2), and chemisorbed oxygen (COOH carboxylic groups) (O-3), respectively.48,49 The following reactions of electroactive functional surface groups could be considered:41,50
C–OH + OH− ⇔ CO + H2O + e− | (1) |
–COOH + OH− ⇔ –COO− + H2O + e− | (2) |
Sample | Element content from XPS (at%) | % of total N 1s | % of total O 1s | ||||||
---|---|---|---|---|---|---|---|---|---|
C | N | O | N-6 | N-5 | N-Q | O-1 | O-2 | O-3 | |
a Pyridinic nitrogen (N-6), pyrrolic nitrogen (N-5), quaternary-N (N-Q). CO quinone type groups (O-1), C–OH phenol groups and/or C–O–C ether groups (O-2), and chemisorbed oxygen (COOH carboxylic groups) (O-3). | |||||||||
HHCSs-600 | 81.9 | 7.4 | 10.7 | 37.5 | 16.4 | 46.1 | 35.9 | 46.8 | 17.3 |
HHCSs-700 | 83.4 | 7.3 | 9.3 | 28.2 | 16.6 | 55.1 | 29.7 | 36.3 | 34.0 |
HHCSs-800 | 88.3 | 4.8 | 6.9 | 8.5 | 45.3 | 46.2 | 18.9 | 48.2 | 32.8 |
In alkaline electrolytes, quinone groups are not electrochemically active, but carboxyl/phenol groups can react with OH− to provide pseudocapacitance.50–52 Hydroxyl groups and carboxyl groups have been found to be effective in improving carbon wettability and beneficial for electrolyte infiltration of the electrode. These two factors can improve the electrode capacitance and rate capability.5,53
XPS quantitative analysis reveals that the contents for nitrogen and oxygen species in HHCSs intensively depend on the pyrolysis temperature (see Fig. 4 and Table 1). When the pyrolysis temperature was increased from 600 to 800 °C, the heteroatom content decreased. As shown in Table 1, despite their different pyrolysis temperatures, all HHCSs possess a relatively higher amount of N-Q than N-5 and N-6 species. The content of N-6 decreases with the increase of pyrolysis temperature, especially between 700 °C and 800 °C, which is consistent with the previously reported studies.54,55 Moreover, the content of O-1 decreases with the increase of pyrolysis temperature.
Fig. 4 N 1s spectra of (a) HHCSs-600, (b) HHCSs-700 and (c) HHCSs-800; O 1s spectra of (d) HHCSs-600, (e) HHCSs-700 and (f) HHCSs-800. |
The specific surface area and porous properties are important for the electrode materials used in supercapacitors. The N2 adsorption/desorption isotherms of HHCSs were shown in Fig. 5. The distinct hysteresis loops were found in the adsorption/desorption isotherms of HHCSs-600 and HHCSs-700, indicating the existence of mesoporous and microporous structures for HHCSs-600 and HHCSs-700. Table 2 shows that the HHCSs-700 possesses the highest surface areas and pore volume. Besides, it is found that HHCSs-800 possesses the lowest surface areas and pore volume. The decrease of surface areas in HHCSs-800 is due to the collapse of pores occurred at relatively high temperature. The specific surface area of the HHCSs-700 is 253 m2 g−1 and the total pore volume is 0.26 cm3 g−1. This can facilitate effective ion diffusion for the electrode.34–36 The micropores of the HHCSs are favorable for enlarging the specific surface area, and mesopores offer larger channels for liquid electrolyte access and ion transport.
Samples | SBET (m2 g−1) | Vpore (cm3 g−1) | St-potmicro (m2 g−1) |
---|---|---|---|
HHCSs-600 | 199 | 0.19 | 153 |
HHCSs-700 | 253 | 0.26 | 191 |
HHCSs-800 | 26 | 0.13 | 5 |
Fig. 6a shows the CV curves of the HHCSs over a potential range from −0.8 to 0 V with a scanning rate of 50 mV s−1. All the CV curves of HHCSs show rectangular-like shapes with broad redox peaks at low potentials, indicating that the electrodes possess both EDLC and faradaic capacitance.56 The CV curves revealed that HHCSs-700 possessed the relatively highest specific capacitance because of its high heteroatoms content and high specific surface area. Fig. 6b shows the characteristic galvanostatic charge/discharge curves of HHCSs at the density of 0.5 A g−1. The galvanostatic charge/discharge curves of HHCSs are not isosceles triangle due to the existence of pseudocapacitance. The specific capacitance of the HHCSs was evaluated according to the discharge time of galvanostatic charge/discharge. The discharge time of HHCSs-700 electrode is longer than that of HHCSs-600 and HHCSs-800 electrodes, indicating that HHCSs-700 possessed the relatively highest specific capacitance. The specific capacitances of HHCSs were calculated from galvanostatic discharge curves, and the comparison of the capacitance retention for HHCSs at a current density range from 0.5 to 10 A g−1 is presented in Fig. 6c. At a current density of 0.5 A g−1, specific capacitances of 192, 241 and 67 F g−1 are obtained for HHCSs-600, HHCSs-700 and HHCSs-800 electrodes, respectively. The specific capacitance of HHCSs-700 is higher than that of the heteroatoms-doped carbon materials at the same current density.15,33,34,42,43 To evaluate the cycle life of the HHCSs-700 for practical applications, the change of specific capacitance versus cycle number for the HHCSs-700 at a current density of 10 A g−1 is presented in Fig. 6d. Owing to the irreversible chemical reaction, the capacitance of HHCSs-700 decreases 8.5% after 10 cycles, but the capacitance decreases by only 3.6% after 10000 cycles, indicating good cycling stability as an EDLC electrode material. The excellent performance of HHCSs-700 is attributed to the combination of hollow spherical porous structure and the heteroatoms-doped carbon framework.22,55
EIS analysis is a powerful and informative technique to evaluate the properties of conductivity, structure and charge transport in the electrolyte interface.57 Fig. 7 gives the curves of Nyquist plots of HHCSs electrodes in 6 M KOH aqueous solution. In the low-frequency region, HHCSs-700 electrode shows nearly a vertical line with higher slop suggesting that HHCSs-700 electrode has a Warburg resistance of charge saturation.58 The slope of 45° portion of the curve in the medium frequency region indicates the characteristic of ion diffusion in the electrode structure. And the quasi-semicircle at high frequency suggests the charge-transfer resistance at the electrode–electrolyte interface. The charge transfer resistance of HHCSs-700 is extremely low from depressed semicircles, showing better capacitor behaviours.59 The smaller impedances imply that the unique hollow nanostructure with well-developed porosity may facilitate fast ion and electrical charge transfer.
Fig. 7 Nyquist plots of HHCSs electrodes (the inset shows the expanded high-frequency region of the plots). |