Chan Hyuk Ji,
Ji Young Lee,
Kee Tae Kim and
Se Young Oh*
Dept. of Chemical and Biomolecular Engineering, Sogang University, Seoul 04107, Republic of Korea. E-mail: syoh@sogang.ac.kr
First published on 23rd September 2019
To achieve high detectivity of organic photodetectors (OPDs), we investigated hafnium oxide (HfO2) as an electron blocking layer in an attempt to obtain a low leakage current and high photocurrent by the tunneling effect. The prepared devices consisted of indium tin oxide (ITO)/HfO2/(poly(3-hexylthiophene-2,5-diyl)[P3HT]:PC60BM)/Yb/Al. To explore the tunneling effect in a hafnium oxide thin film, we fabricated a thin film using successive ionic layer deposition. The results for hafnium oxide were compared with those for aluminum oxide and poly(3,4-ethylenedioxythiophene)poly(styrenesulfonate) (PEDOT:PSS). We found that hafnium oxide results in a low leakage current and high photocurrent owing to the tunneling effect in the OPDs. The resulting detectivity of 1.76 × 1012 Jones for a film thickness of 5.5 nm and bandwidth of ∼100 kHz is suitable for commercialization.
One of the most important parameters for OPD performance is detectivity, which is also affected by leakage current.9 The leakage current in OPDs has been improved by blocking electrons sourced from the external bias. The electrons are blocked by an interlayer composed of a high work function material, and holes are blocked by a cathode interlayer with a low work function.10,11 The electron blocking layers serve to block leakage current under a reverse bias and extract photo-generated carriers from the active layer to the electrode, whereas the hole blocking layer is supported by an external bias and reduced charge recombination in the active layer.12 For a p-type buffer layer, PEDOT:PSS [poly(3,4-ethylenedioxythiophene)poly(styrenesulfonate)] has been widely used as a hole transporting material. However, OPDs using a PEDOT:PSS layer contend with problems involving high dark current densities from leakage current and poor device stability.13 In this study, we introduced thin film of hafnium oxide as an electron blocking layer to reduce the dark current density caused by the leakage current and improved the on–off current ratio and detectivity. To understand and the effective thickness of hafnium oxide layer for low leakage current and tunneling effect, we applied successive ionic layer deposition (SILD)14,15 as hafnium thin film fabrication technique which can be deposited less than 4 nm thickness film. Hafnium oxide has a high bandgap (5.0–6.0 eV) and can control leakage currents, making it widely used as an insulator in semiconductor industries.16,17 In addition, hafnium oxide is an effective material for blocking carriers owing to its characteristics as an insulator. In a ∼5 nm thin film, tunneling can happen in certain device configurations18,19 and has been shown to occur in OPD devices.
Herein, we demonstrate OPDs with high detectivity using hafnium oxide in an ITO/HfO2/P3HT:PC60BM/Yb/Al configuration. To fabricate hafnium oxide thin films, 2.0 nm, 5.5 nm and 11 nm layer of hafnium oxide was deposited by SILD.14,15 Hafnium oxide, PEDOT:PSS, and aluminum oxide were compared as electron blocking layers to understand and analyze the reason for the low dark current and the effect of tunneling in the OPD device by selection of similar energy level metal oxides, and ytterbium was used as the electron transport layer for a high photocurrent.20 Using the hafnium oxide in the OPD devices as an electron blocking layer, we found that the hafnium oxide thin film in the OPD device controls the dark current by blocking external bias under a wide bandgap and high lowest unoccupied molecular orbital (LUMO) level in the dark state; furthermore, it enhances the photocurrent by way of the tunneling effect in the light state, as confirmed by comparison with aluminum oxide, which has a similar wide band gap and LUMO level.
In the first step, well-cleaned patterned ITO glass substrate was immersed for 20 seconds in the cationic precursor solution of hafnium chloride. The hafnium ions get adsorbed to the surface of the substrate. Afterwards, the substrate was rinsed for 20 seconds by DI-water to remove excessively adsorbed ions.
In the second step, the substrate was immersed for 20 seconds in the anionic precursor solution of hydroperoxide. The hydroxide ions react with adsorbed hafnium ions on the substrate to form HfO−. The substrate was rinsed for 20 seconds by DI-water to remove excessive substrate again.
The above two steps together constitute one complete cycle of deposition. This cycle was repeated several times to get well adhesiveness and homogeneous HfO2 thin layers. Finally, annealed at 400 °C for 30 minutes in a furnace for the perfect oxidation of HfO2 thin film. OPD devices consisting of ITO (200 nm)/HfO2/P3HT:PC60BM (210 nm)/Yb (2 nm)/Al (100 nm) were fabricated on the hafnium oxide thin film deposited ITO glass. The device was transferred into a nitrogen filled glove box where a solution of P3HT:PC60BM (1:1) in dichlorobenzene (36 mg ml−1) was spin-cast at 900 rpm onto the hafnium oxide thin film and annealed at 120 °C for 10 minutes on a hot plate. Finally, ytterbium and aluminum were deposited by using a thermal evaporation technique at 10−6 torr (ULVAC VTR-300M/1ERH evaporator, Japan).
Table 1 and Fig. 3 show the current density–voltage characteristics of the OPDs with different hafnium oxide thin film thicknesses as the electron blocking layer. The photocurrent and dark current density decreased proportionally to the thickness of the hafnium oxide film, confirming that a high hafnium oxide LUMO level can act as a high energy barrier between the ITO electrode and active layer.
Thickness (nm) | Hafnium wt% (FE-SEM) | Photocurrent density (A cm−2) | Dark current density (A cm−2) | On–off current ratio |
---|---|---|---|---|
2.0 | 0.47 | 6.97 × 10−3 | 3.02 × 10−7 | 2.31 × 104 |
5.5 | 1.04 | 5.27 × 10−3 | 4.15 × 10−8 | 1.27 × 105 |
11 | 4.06 | 5.66 × 10−5 | 3.31 × 10−8 | 1.71 × 103 |
Fig. 3 Current density–voltage curves of organic photodetector devices (OPDs) with various hafnium oxide electron blocking layer thicknesses. |
We found that at a thickness of 5.5 nm, electrons passed through the hafnium oxide thin film, and its electron blocking effect decreased dramatically. Photocurrent density and dark current density tended to be inversely proportional to hafnium oxide thickness. However, when the thickness was 5.5 nm, accumulated holes in the active layer owing to the HOMO level of hafnium oxide caused energy band bending, leading to quantum tunneling and extraction of holes to the ITO electrode.18 The highest on–off current ratio of 1.27 × 105 was observed for the OPD with 5.5 nm of hafnium oxide.
Fig. 4 Energy diagram of organic photodetector devices (OPDs) with three different electron blocking layers. |
The current density–voltage characteristics of the prepared OPDs with different electron blocking layers are presented in Table 2 and Fig. 5. Their dark current densities were 4.15 × 10−8 A cm−2 at 5.5 nm of hafnium oxide, 3.53 × 10−8 A cm−2 at 6.0 nm of aluminum oxide, and 1.11 × 10−7 A cm−2 at 30 nm of PEDOT:PSS. The dark current density was reduced by the prevention of electron injection from the ITO electrode by the hafnium oxide thin layer. On the other hand, hafnium oxide at a certain thickness can transfer the photo-generated carriers produced by tunneling effects from the active layer. Thus, it can be argued that a hafnium oxide thin layer can behave as a hole transport material owing to the tunneling effect.
Material | Thickness (nm) | Photo current density (A cm−2) | Dark current density (A cm−2) | On–off current ratio | Detectivity (Jones, at 520 nm) |
---|---|---|---|---|---|
HfO2 | 5.5 | 5.27 × 10−3 | 4.15 × 10−8 | 1.27 × 105 | 1.76 × 1012 |
Al2O3 | 6.0 | 7.51 × 10−7 | 3.53 × 10−8 | 2.13 × 101 | 9.16 × 1010 |
PEDOT:PSS | 30 | 8.26 × 10−3 | 5.00 × 10−6 | 1.60 × 103 | 2.01 × 1011 |
Fig. 5 Current–voltage curves of organic photodetector devices (OPDs) with different electron blocking layer materials. |
However, the HOMO–LUMO levels of hafnium oxide and aluminum oxide are similar, and their current density–voltage characteristics in our OPD configurations under a reverse bias were dissimilar. It seems that tunneling could happen in film thicknesses of 5.5 nm and 3 nm for hafnium oxide and aluminum oxide, respectively (see Table S1†). As shown in Table 1, 5.5 nm is the optimized hafnium oxide thickness for a low dark current and high photocurrent. In contrast, for aluminum oxide, the tunneling effect would occur in a thinner film, and the increase in photocurrent density would thus be limited in terms of significantly increasing the on–off ratio. However, aluminum oxide showed a comparably low photocurrent density in the OPD configuration owing to its relatively low capacitance,23 and thus it exhibited low charge accumulation and tunneling in the OPD configuration.
Fig. 6 shows the external quantum efficiencies (EQEs) at different wavelengths under reverse bias conditions at −1 V of the optimized OPDs using hafnium oxide, aluminum oxide, and PEDOT:PSS as electron blocking layers. All the OPDs showed photo-responses from 300 to 800 nm. At wavelengths of 300–400 nm, the EQE of the OPD using PEDOT:PSS was higher than that of the metal oxide based devices. In particular, the EQE of the hafnium oxide based OPD was higher than that of the PEDOT:PSS OPD at 400–600 nm, which was attributed to the high transmittance. The aluminum oxide based OPD showed very low EQEs over the whole range of wavelengths because the generated holes in the photoactive layer could not be effectively extracted to the electrode. High transmittance of hafnium oxide was expected in the visible range as the absorption was insignificant for wavelengths above 250 nm.24 The higher transmittance of hafnium oxide can detect light effectively in the visible rage, it is presented in the Fig. 7.
Fig. 6 External quantum efficiencies (EQEs) of different organic photodetector devices (OPDs) with different electron blocking layer materials. |
Responsivity (R), NEP (λ) and detectivity (D*) are the most important parameters in terms of OPD performance and can be calculated given the EQE. The detectivity is related to the responsibility and noise-equivalent power (NEP). The reciprocal of the NEP (Noise-Equivalent Power) is referred to as the detectivity of the device:20
(1) |
(2) |
(3) |
Fig. 8 Frequency responses of optimized organic photodetector devices (OPDs) using hafnium oxide and poly(3,4-ethylenedioxythiophene)poly(styrenesulfonate) (PEDOT:PSS) interlayers at −1 V. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra06230k |
This journal is © The Royal Society of Chemistry 2019 |