Karthik
Raghunathan‡
a,
Jibin
Antony‡
b,
Sarmad
Munir
c,
Jens-Petter
Andreassen
b and
Sulalit
Bandyopadhyay
*b
aUgelstad Laboratory, Department of Chemical Engineering, Norwegian University of Science and Technology, N-7491, Trondheim, Norway
bDepartment of Chemical Engineering, Norwegian University of Science and Technology, N-7491, Trondheim, Norway. E-mail: sulalit.bandyopadhyay@ntnu.no
cYara International ASA, Herøya Research Park, Hydrovegen 67, 3936, Porsgrunn, Norway
First published on 25th March 2020
Synthesis of gold nanorods (Au NRs) using surfactant-mediated seeded growth involves the interplay of parameters such as pH, reducing agent, and surfactant among others. The use of binary surfactant mixtures of cetyltrimethylammonium bromide (CTAB) and oleic acid (OA) has been reported by our group previously to obtain other anisotropic shapes. However, there are no reports investigating the growth kinetics and mechanisms of such shapes. Here, we report for the first time a ternary representation for compact visualization of shape transitions of gold nanoparticles (Au NPs) as a function of reaction parameters. Further, using UV-Vis spectrophotometry, the growth kinetics of these shapes was tracked using an in-house developed technique. The interplay between the experimental parameters and the properties of Au NPs was investigated using statistical analysis which showed that the reducing agent and pH were significant in influencing shape and growth kinetics. We further propose a growth mechanism in which the supersaturation of growth units controls the final shapes obtained.
Among other synthesis methods, seed-mediated growth in the presence of cetyltrimethylammonium bromide (CTAB), developed by Jana et al.,13 has garnered considerable interest among researchers since its inception, due to the ease and robustness with which it can induce shape control. This method involves the growth of NPs in supersaturated growth solutions by introducing a seed solution. A number of modifications have been employed in this method in order to achieve better shape selectivity. Nikoobakht et al. performed experiments by adjusting the silver content of the growth solution in order to obtain nanorods (NRs) with controlled Aspect Ratios (ARs).14 The pH of the growth solution, being an important parameter in determining the reduction potential of the reducing agent (ascorbic acid (AsA)), has been shown to have a significant effect on the shape of Au NPs.15,16 Studies performed by Okitsu et al. report a substantial decrease in the AR of Au NRs with an increase in the pH of the growth solution, with shapes resembling spheres at pH 9.8.15 Though a few mechanisms were suggested by the authors, the small experimental dataset limited their conclusiveness, thus highlighting the need for a more systematic study. More recently, the growth process has been explained using supersaturation of the growth units as an important parameter to control the exposed crystal faces of the NPs, thereby affecting their shape.17
Investigating the growth kinetics of anisotropic NPs would lead to a better understanding of the shape evolution. The kinetics of a silver-mediated Au NR system was studied by Bullen et al. using UV-visible spectrophotometry, and they report the growth rate to be dependent on the concentration of the reducing ascorbate monoanion and pH around the pKa of AsA.18 A few other studies examining the growth kinetics of Au NRs include the use of small-angle X-ray scattering (SAXS)19 and atomic force microscopy coupled with electron microscopy of surface-bound NPs.20 However, the datasets, being relatively small, are not representative of the studied sample space, thereby preventing statistically significant analysis of growth and the associated kinetics. Additionally, there is no report on understanding the growth kinetics for Au NPs of different shapes, as most of these studies primarily focus on Au NRs. On the contrary, various hypotheses have been reported in the literature to explain the possible mechanisms that lead to the growth of anisotropic NRs from the initial spherical gold seeds.21–23 A recent investigation by Edgar et al. suggested a stochastic growth mechanism for Au NRs, where different seeds grow non-uniformly to attain the final NR shape.24 Performing statistical studies for identifying the most critical parameters in NP formation could provide precise control of Au NP surface chemistry, thereby giving better yields. A recent study reported by the Murphy group used a fractional factorial design of experiments to understand the important experimental variables and quantify their effects when synthesizing Au NRs.25 However, the study was limited only to Au NRs.
The primary focus in seeded growth is the use of the single surfactant CTAB and all the above studies have shed light on understanding shape control, kinetics and/or mechanistic insights for such a process. The presence of an additional co-surfactant in seed-mediated growth has been reported to significantly improve the dimensional tunability. The effect of binary surfactant mixtures of CTAB with oleyl functional groups such as sodium oleate (NaOL), sodium linoleate and oleylamine on the shape tunability of Au NRs was investigated by Ye et al.26 A further extension of this work, studying the overgrowth of Au NRs, by Khlebtsov et al. also reported dimensional and plasmonic tunability of Au NRs using binary surfactant mixtures of CTAB and NaOL.27 Previous work carried out by our group demonstrated shape tunable synthesis of anisotropic Au NPs through the use of binary surfactant mixtures of didodecyldimethylammonium bromide (DDAB) and CTAB.28 However, the scope of these studies was limited to changes in a few synthesis variables and they did not delve into the growth mechanism or kinetics of growth. To our knowledge there are no reports of a systematic study investigating the growth and growth kinetics of different anisotropic shapes of Au NPs involving binary surfactant mixtures. An additional challenge while employing a secondary surfactant is an increase of one more reaction parameter that can be varied to control the growth in addition to the studied parameters as in the case of a single surfactant system. This calls for better visualization of the data space in order to map the morphological transitions from one shape to another. An effective tool to accomplish this is a ternary representation which has been commonly used in other research domains.
Here, we report for the first time a ternary representation of the data space for a compact visualization of shape transitions of Au NPs as a function of reaction parameters. We also study and report for the first time the growth and growth kinetics of different anisotropic shapes of Au NPs by varying the pH, amount of the reducing agent, and seed type among other factors in seed-mediated growth employing binary surfactant mixtures of CTAB and oleic acid (OA). Multivariate linear regression analysis is performed on the experimental dataset to determine statistically significant variables for shape control of Au NPs. The kinetics studies coupled with the statistical analysis enable us to understand and provide insights into the growth mechanism that is postulated from a classical nucleation standpoint as a function of supersaturation of growth units.
A wide array of anisotropic Au NPs has been synthesized in this study employing the seed-mediated growth strategy. Herein, two different Au seeds – CTAB coated and Na-citrate coated seeds – have been used to investigate the growth of anisotropic Au NPs synthesized via single and double seeding as outlined below. Characterization of the anisotropic Au NPs, kinetic studies to investigate their growth mechanisms and statistical analysis to understand and evaluate trends in data sets were carried out and are discussed in the subsequent sections.
The CTAB or citrate coated seeds were used for the growth of anisotropic NPs without further purification.
The experimental process for single-seeded growth is described herein. 1.2 g of CTAB and varying amounts of the co-surfactant, OA (Table S1†), were dissolved in 15 ml of MQ water (80 °C) via vigorous stirring (1200 rpm). After the solution turned transparent, the temperature was lowered to 35 °C. Thereafter, 750 μl of a freshly prepared 4 mM AgNO3 solution was added to the surfactant mixture and stirred for 15 min at 35 °C. This was followed by addition of 15 ml of 0.86 mM HAuCl4·3H2O and the solution was further stirred for 15 min at the same temperature. If required, the pH of the solution was adjusted at this stage using different volumes of either 1 M HCl or 0.1/0.01 M NaOH. Thereafter, different volumes of 128 mM AsA (Table S1†) were added to the reaction mixture followed by stirring at 1000 rpm to obtain a colourless solution. The disappearance of the colour indicates the reduction of Au3+ to Au1+.13,28 For the single-seeded experiments, 96 μl of the Au seed solution (CTAB or citrate coated) was finally added to the growth solution under vigorous stirring (1200 rpm). In the case of double seeded experiments, an intermediate growth solution was prepared using the protocol outlined above (with 30 μl OA and identical steps afterwards), ending with the addition of 96 μl of the Au seeds (CTAB coated). The name double-seeded is coined based on the fact that after 30 s, 300 μl of this intermediate growth solution was used as a seed for further growth in fresh growth solutions.
For both single and double-seeded experiments, after 30 s of the addition of the seeds into the growth solution, stirring was stopped, and the resultant reaction mixture was left for 8 h at 35 °C for completion of the reaction. Thereafter, the reaction mixture was centrifuged twice at 11000 rpm for 20 min and the Au NPs were re-dispersed in 5 ml of MQ water.
Detailed information about the experimental conditions used for the synthesis of Au NPs is reported in Table S1.†
UV-Vis spectra for studying the growth kinetics and obtaining the plasmonic peaks of the NPs were acquired using a UV-2401PC (Shimadzu) spectrophotometer. The spectra were collected over a spectral range from 400–900 nm.
In the current study, 3.5 ml of the growth solution was immediately withdrawn after addition of seeds and transferred into a UV-Vis cuvette (disposable cuvette from PLASTIBRAND®). The instrument was also maintained under the reaction conditions (35 °C). The time difference from sample withdrawal until the start of spectral acquisition was noted to be approximately 30 s for each experiment. This time lag in acquiring spectra was compensated for during analysis of the kinetic data. UV-Vis spectra in the range 400–900 nm were obtained for 2.5–6 hours (longer time for lower pH samples) by using the UV-Vis repeat mode, in which the instrument continuously measures absorbance over time.
The UV-Vis instrument can measure the absorbance of metallic Au0 that is formed upon addition of seeds due to an autocatalysis reaction involving Au1+ following first-order kinetics.18,24 The area under the spectrum gives a measure of the total quantity of Au0 formed from the available Au1+ in the solution upon addition of seeds. With time, the areas under the curves increase monotonically until they are saturated. Individual areas obtained for a single type of NP were normalized against the area of its final spectrum obtained at the end of UV-Vis measurements for ease of quantitative analysis. The curve between the normalized area and reaction time was fitted with the sigmoidal 4 parameter equation given below and the first-order rate constant was calculated using the fitting parameters.
(1) |
Fig. 2(a) shows an overview of the different shapes of Au NPs that were obtained under the different synthesis conditions employed in the current study. We report for the first time a ternary space representation as a tool for showing morphological transitions of anisotropic Au NPs as a function of reaction parameters. The ternary space diagram shows the variation of the shapes as a function of three normalized parameters – (i) the volume ratio of OA to AsA , (ii) the volume ratio of silver nitrate to CTAB coated seeds and (iii) the scaled pH of the solution after addition of AsA . The synthesis parameters are grouped based on the fact that both OA and AsA play the role of reducing agents, while AgNO3 and seeds are known to play important roles in determining anisotropic growth. It should, however, be noted that each of the above parameters has been normalized to its respective highest value followed by utilization of ternary transform in SigmaPlot that normalizes the data to a ternary space for the sake of better visualization of morphological transitions. A first glimpse at the ternary space shows that a large number of shapes can be synthesized ranging from spheres to NRs, etched nanorods (ERs), tetrahexahedra (THH), multifaceted structures, and the recently reported nanomakura (NM).30 Another important reason to convert the dataset into a ternary space diagram is the ease with which the varying parameters can be studied to account for the morphological changes in the obtained shapes along different connecting lines. This shall enable a qualitative understanding of the role of various synthetic parameters in affecting the shape transitions of Au NPs. Thus, the ternary space plots shown here only provide a visual means to group and classify various morphologies as a function of reaction parameters, as opposed to representing thermodynamical phase equilibria as in ternary phase plots.
In order to understand the effect of varying parameters on shapes, a set of connecting lines (a, b, c and d) are used in Fig. 2(a). Along line ‘a’, as the pH increases, the morphology of the Au NPs changes from NR → ER → sphere. For another line ‘b’, if the pH increases, the shapes change as follows: THH → NM → multifaceted sphere. Both lines show that an increase in pH of the reaction medium results in the formation of structures with an increasing number of facets. An increase in pH can be equated to an increase in the strength of the primary reducing agent (AsA) affecting the overall growth kinetics. On the other hand, an increasing does not change the morphology of the Au NPs, represented by the line ‘c’. This line shows that NM is formed as the only morphology under these conditions. However, the line ‘d’ represents the fact that increasing changes the morphology from NR → ER. Thus, an interesting observation from lines ‘c’ and ‘d’ is the fact that OA or AsA has a comparatively lower effect on the morphology of the obtained NPs when the pH is appropriately tuned. Overall, pH seems to have a dominating role in controlling the growth of these NPs. Interestingly, a large number of points coincide on the scaled vertex of the ternary plot. In order to have a closer look at the morphologies involved, a separate ternary plot is drawn in Fig. 2(b) for OA = 0.
As can be seen from Fig. 2(b), even without the use of OA, it is possible to synthesize a plethora of shapes ranging from NSs, NRs, and ERs to multifaceted structures. However, there are clear zones in the plot where NRs and ERs lie, indicating that appropriate tuning of the synthesis parameters is an essential aspect for shape control. On the other hand, the absence of AgNO3 (represented by the base of the ternary plot opposite the vertex) hampers the selectivity of one shape over other shapes in the final product. However, this selectivity can be tuned by adjusting AsA and pH. An increase in pH coupled with a decrease in AsA leads to the formation of longer NRs and spheres via several other shapes that include prisms and multifaceted structures.
In a typical synthesis protocol (without the use of a co-surfactant), the yellow coloured growth solution turns colourless upon addition of the primary reducing agent, AsA. This is an indication of the complete conversion of Au3+ to Au1+. In the case of our experiments, the pH of the growth solution was adjusted before the addition of AsA via using NaOH or HCl. The pH values reported were measured after the addition of AsA and before the addition of the seed. It is worth mentioning that the growth solution decolourized even before the addition of AsA when OA was present in the reaction mixture. This happened more noticeably when increasing the pH, pointing once again to the fact that pH is a significant variable for growth control.
Fig. 3 Effect of pH on the shape of Au NPs. (a–i) Representative S(T)EM images of different Au NPs (pH after adding AsA). |
In the absence of AgNO3, increasing the pH results in better shape selectivity (compare Fig. 3(a) and (c)). Upon addition of AgNO3, improved shape selectivities can be observed under both low and high pH conditions. At low pH (∼1.5), addition of AgNO3 leads predominantly to NRs with an AR of 3.2 ± 2.0 (L = 42 ± 13 nm, D = 16 ± 6 nm, Fig. 3(d)). Smoother and higher AR NRs (3.9 ± 1.2, Fig. 3(g)) are obtained upon addition of OA. At high pH (∼7), addition of AgNO3 leads predominantly to ERs with an AR of 2.8 ± 1.0 (L = 36 ± 7 nm, D = 15 ± 5 nm, Fig. 3(f)). Addition of OA leads to the formation of spheres of size 18 ± 3 nm (Fig. 3(i)).
At low pH (∼1.5), in the presence of OA, NRs are obtained as discussed above. A similar morphology can be observed in the case of pH 3 in the absence of OA (Fig. 3(e)). When one compares Fig. 3(h) and (f), similar morphologies, i.e. ERs can be observed. Therefore, by adjusting either the pH or the amount of OA, finer control over the morphology of the obtained Au NPs can be exerted.
An increase in pH, however, promotes shape selectivity, resulting in more spheres and NRs, in comparison to other shapes (Fig. 3(c)). However, in the absence of AgNO3, a certain degree of shape selectivity can be achieved. As the pH increases, the standard deviation of the long axis of the NPs goes down from 75 nm to 24 nm as the number of different/irregular shapes obtained decreases. In the presence of AgNO3, shape selectivity is achieved, and uniform anisotropic NPs are obtained. At low pH, NRs of different sizes are obtained, and uniform NRs are obtained when the pH is unaltered (pH = 3). As the pH increases, the size of NRs decreases and at pH 7.2, the shapes change to ERs.
Two different seeding techniques have been employed – single seeding and double seeding. In the latter case, intermediate growth solutions were added as seeds to fresh growth solutions. Our group were the first to report the shape nanomakura obtained under such conditions.30 However, when the pH is varied, a transition from THH NPs to multifaceted sphere-like NPs is observed (Fig. S9†). This trend of shape transition is similar to the trend observed for single seeding with OA where a shape transition occurs from NRs to ERs to spheres under similar conditions. pH also affects the reducing capability of AsA, which is then expected to exert an influence on the morphologies obtained.
Fig. 4 Effect of ascorbic acid on the shape of Au NPs. (a–e) Representative S(T)EM images of different Au NPs. |
Conversely, in the absence of AgNO3 and OA (Fig. 4(a) and (d)), different shapes were obtained. However, the shape selectivity of NRs and spheres over other shapes improved on increasing the amount of AsA. In the presence of AgNO3, at 135 μl of AsA (Fig. 4(c)), uniform NRs (AR 3.2 ± 1, length 40.2 ± 7.7 nm) were obtained. When the amount of AsA is increased, the obtained shapes changed from NRs to ERs – a representative ER (AR 3.0 ± 0.8, length 39.4 ± 6.1 nm) at the highest amount of AsA is shown in Fig. 4(b).
In order to understand semi-quantitatively the influence of reaction parameters on the shapes of the obtained Au NPs, the growth of the Au NPs was followed using UV-Vis spectrophotometry.
The same procedure was followed for different reaction conditions such as with and without AgNO3, with OA and double seeding which yield random shapes, NRs, ERs and NMs, respectively. Fig. 5(c) shows the normalized areas under the curves obtained for these different conditions. High values (∼1) of regression coefficients show that the fitted curves are a statistical representation of the growth kinetics. The sigmoidal nature of the curve in all the above cases indicates that the reaction is autocatalytic for all the studied conditions. Similar autocatalytic growth of NRs has been reported previously.24,25,31 There is an initial slow growth phase, characteristic of sigmoidal growth, for all the shapes; however, the exponential growth phase starts at increasing time points for samples without AgNO3 followed by samples with OA, further followed by samples with AgNO3 and finally double seeded samples. These time points are in coherence with the time points at which a visible colour change occurs (for all samples). Our observation is in line with previous reports, where the role of AgNO3 in retarding growth kinetics is well established.18,23 Further, we observe that the addition of OA shortens the growth lag, indicating the role of OA as a reducing agent, as discussed before. In the case of the double seeded experiments, the amount of OA used is higher; however, there is retarded growth kinetics in comparison to the other shapes. As reported previously by our group, the seeds, in this case, are not homogeneous (different shapes),30 which can explain the presence of different shapes in the growing media, further supported by broad UV-Vis peaks that continue to grow temporally. Therefore, the spectral signatures of individual axes are masked by the broad shape distribution present at all times.
A single UV-Vis run for the whole wavelength range (400–900 nm) takes ∼90–100 seconds resulting in the loss of temporal data points leading to a loss of kinetic information in the initial phase of the reaction. To verify the effect of the increased number of time points, UV-Vis measurements were performed for smaller wavelength ranges for NRs and ERs. The fitting parameters obtained for the longitudinal and transverse axes in our representative datasets were comparable to the fitting parameters obtained for the whole wavelength range (400–900 nm) (Table S4†). In addition, the fitting parameter representative of kinetics (b from eqn (1)) of the longitudinal axis represents the fitting parameter (b from eqn (1)) obtained for the whole wavelength range. Therefore, once the locations of the LSPR peaks of the desired shape are known, a smaller range wavelength scan around the LSPR will be advantageous to facilitate data collection for an increased number of time points. This will lead to higher accuracy in the capture of the kinetics of faster-growing shapes, especially in the initial growth phase. Further, since we have shown that small range scans provide representative fitting parameters for the overall growth kinetics, these can be used for understanding the overall growth kinetics.
The first-order rate constants (k values) obtained for these conditions are shown as a part of Fig. 5(d). These complement the ongoing discussion about the role of AgNO3 and OA in kinetics, where their addition retards the overall kinetics. The experiments with AgNO3 show slower kinetics than the ones with OA. The reported k values are obtained averages from three different repeats for each condition. The low standard deviations indicate the reproducibility of this method for determining growth kinetics of anisotropic shapes. Since this method uses UV-Vis spectrophotometry and we have shown applicability for different shapes, we believe our method can be expanded to follow the growth of other shapes yielding information about the growth kinetics.
Correlation loadings (Fig. S10–S12†) using the partial least squares method show the statistical importance of different reaction parameters for shape tunability. AgNO3 is shown to be statistically significant in influencing shape selectivity. Further, the need for OA to obtain ERs when parameters such as pH and amount of AsA are kept constant is also evident. Our findings strongly suggest that for better control of kinetics and for fine-tuning of shapes in a seeded growth method employing binary surfactant mixtures, a one-day shelf life is recommended for AsA and AgNO3.
Therefore, in designing our experimental matrix, where we investigate the effects of pH, AsA, OA, type of seed and other reaction parameters, we have used the guidelines for chemicals as indicated by our correlation loadings study. The synthesis of Au NPs using a seeded growth method requires a complex mixture of both thermodynamic and kinetic controls, resulting in a large number of parameters to be studied. This necessitates a multivariate approach to understand their roles in controlling the growth kinetics leading to different shapes.
Here, we report for the first time that the presence of OA in the growth medium decreases the overall growth rate showing that OA has a retarding role in controlling the growth kinetics. Previous reports have shown that the presence of AgNO3 in the growth medium slows down the kinetics.18 Our findings in growth kinetics determined using the UV-Vis methodology also reflect the same. On the other hand, the overall growth rates increase when the pH of the growth medium or amount of AsA is increased. Among other factors, the growth rate is influenced largely by the reduction rate of Au1+ (reduction product of Au3+, the reduction achieved in the synthesis process using AsA) to Au0, which is dependent on the reduction environment. An increase in the reduction rate can be achieved either by increasing the reduction potential or by increasing the amount of the reducing agent used. At a higher volume of AsA, there is a higher availability of the reducing agent, while an increase in pH above the pKa value of AsA (pKa = 4.7) increases the reduction potential of AsA. These effects, in turn, increase the overall growth rates represented by the increase in the k values. Although the change in pH or AsA results in similar effects, it is important to emphasize the dominant role of pH in controlling growth rates besides the formation of different shapes, as depicted in ternary space representation. In the case of the effect of pH in the presence of OA, the growth rate constants increase by one order of magnitude when a high pH is maintained. Under similar conditions, different shapes viz. NRs and sphere-like NPs are obtained, as inferred from their LSPR signatures at 761 nm and 520 nm, respectively.
With an aim to statistically interpret the variability in growth kinetics as a function of the reaction parameters, multivariate analysis was performed using JMP to evaluate the interactions among reaction parameters such as pH, amount of AsA, amount of OA, etc. and output response parameters such as physico-chemical properties of Au NPs (like length of the long axis (L), AR, etc.) and the overall growth rate constant. The equation to predict the output response parameter obtained using linear multivariate regression has the following form.
yi = a1x1 + a2x2 + … + anxn + Ci |
y | x | a | c |
---|---|---|---|
k | LSPR | −1.65 × 10−5 | 8.13 × 10−3 |
No. of LSPR peaks | 1.12 × 10−3 | ||
AsA | 4.73 × 10−6 | ||
pH | 4.87 × 10−4 | ||
L | AgNO3 | −6.19 × 10−2 | 5.68 × 101 |
k | −1.31 × 104 | ||
LSPR | 2.23 × 10−1 | ||
AR | −3.78 × 101 | ||
LSPR | OA | 0.127 × 101 | 2.83 × 102 |
AgNO3 | 1.07 × 101 | ||
AsA | 1.30 × 10−1 | ||
No. of LSPR peaks | 4.59 × 101 | ||
L | 9.00 × 10−1 | ||
AR | 5.61 × 101 | ||
No. of LSPR peaks | k | 1.62 × 102 | −0.35 × 101 |
LSPR | 7.76 × 10−3 | ||
AR | OA | −2.44 × 10−2 | 8.24 × 10−1 |
AsA | −1.54 × 10−3 | ||
pH | −2.10 × 10−1 | ||
LSPR | 5.30 × 10−3 | ||
L | −1.07 × 10−2 |
Statistically, k can be predicted as a function of LSPR wavelength, number of LSPR peaks, amount of AsA and pH of the growth solution. pH is also observed to be an important predictor for where the LSPR peak will be located. The LSPR peak position is further dependent on the amount of AgNO3, which is a statistical representation of the fact that AgNO3 plays a dominant role in determining the position of LSPR the peak of the obtained Au NP, thereby affecting shape selectivity, as widely reported in the literature.14,33,34 The plasmonic properties of the Au NPs depend on their shape and size (among other factors); therefore, morphological properties of the NPs like L and AR are found to statistically influence the LSPR peak position. From the previous discussion, the shapes in turn have been shown to depend on experimental parameters such as AsA, OA, AgNO3 and pH. Therefore, the properties of Au NPs like L and AR are dependent on each other (which is similar in the case of LSPR with no. of LSPR peaks) and hence appear as a predictor for one another in the multivariate predictor equations.
The multivariate analysis shows that experimental parameters like pH and amount of reducing agent show a strong correlation with the shapes and growth kinetics of NPs; however, in order to understand the growth mechanism involved, an insight into the role of the different chemicals used and their effects on crystal growth is necessary. From our study, we have observed that the experiments with low AsA (68 μl) lead to a complete reduction of Au3+ to Au1+ after addition of AsA (observable colour change from yellow to colourless of the growth solution), but we observe no growth of the Au seeds under these conditions. This indicates a need for excess AsA for reducing Au1+ to Au0 in the presence of the Au seeds. When the amount of (excess) AsA increases, an increase in the overall growth rate is observed owing to a higher amount of Au0 produced via reduction of Au1+. The k values obtained indicate a similar increasing trend, for example, the k values of experiments with AgNO3 vary from 0 for 68 μl of AsA to 1.94 × 10−3 s−1 at 400 μl of AsA. Interestingly, in experiments with low AsA (68 μl) (which does not result in growth of Au seeds otherwise), ERs were observed, although with slow kinetics (k = 1.48 × 10−3 s−1). This happens because OA also behaves as a reducing agent, owing to the C–C double bond that provides electron density for reduction.35,36 The importance of OA as a reducing agent is further verified through observations in experiments performed under high pH conditions. A colour change from yellow to colourless (of the growth solution), indicating the formation of Au1+ was observed (upon addition of OA) even before the addition of AsA, the primary reducing agent. OA has a pKa of 5.02 and in the case with high pH, the reduction potential of OA is thus expected to increase, leading to the formation of Au1+. The total volume of added AsA, under these conditions, is in excess and helps in the formation of Au0 and leads to a high k value of 6.81 × 10−3 s−1. It is worth mentioning that under these conditions, sphere-like NPs are obtained. Alternatively, at this pH, OA could have reacted with the NaOH used to adjust the pH and resulted in the formation of sodium oleate, another reducing agent with a pKa of 4.99, which was previously shown by Ye et al.26 Sphere-like particles were also obtained at high pH and in the presence of OA for both single and double seeded methods.
Although shape selectivity can be adjusted by altering the pH or AsA, AgNO3 is still an essential requirement to affect the selectivity of one shape over the others. The growth of Au NPs in the surfactant mediated seeded growth method generally follows the following two reduction steps.
Au3+ + e− = Au1+ |
Au1+ + e− = Au0 |
In a typical synthesis (without changing the pH), Au3+ is reduced using the weak reducing agent AsA resulting in a supersaturated solution of Au1+. The second reduction step occurs in the presence of more reductants (excess AsA or secondary reductants) and Au seeds, resulting in the formation of Au0 in the solution close to the surface of the seed. The supersaturated solution of Au0 around the seed forms the driving force for crystal growth. From a crystallization point of view, the growth of these NPs involves the formation of Au0 and integration of the newly formed Au0 on the seeds. However, for the formation of Au0 in the solution, the Au1+ ions have to travel to the surface of the seed where the autocatalytic reaction happens. For a better understanding of the growth, the following steps can be considered schematically.
• Reduction of Au3+ to Au1+.
• Transport of Au1+ to the surface of the seeds.
• Supersaturation of Au0 in solution near the surface of the seeds.
• Surface integration of Au0.
The change in the growth solution from yellow to colourless was observed for all the experiments and a some AsA or a combination of AsA/OA in the system is spent on this reduction step. Due to this colour change, it is assumed that there is a complete formation of Au1+ in all our experiments. A number of mechanisms have been proposed to explain the diffusion of Au1+ by different research groups37–39 and it is not part of the discussion here. Since our main aim is to understand the shape evolution of Au NPs in a binary surfactant system, we focus our discussion on the last two steps, which are crucial for understanding how the CTAB coated Au seeds develop into different morphologies. Therefore, we believe that growth of the anisotropic Au NPs obtained under different experimental conditions can be explained by considering the supersaturation of Au0 in the liquid surrounding the seeds and integration of Au0 on the surface of the seed.
The kinetics of this reaction depends on the amount of reducing agent used and its reduction potential. The Au0 formed as a result of the reduction step creates a localized supersaturation around the seed; however, the concentration of Au0 depends on the amount of AsA available and the pH (indirectly, the reduction potential). At a lower concentration of AsA or low pH, the formation of Au0 is slow, leading to lower supersaturation of Au0. The formed Au0 can therefore easily integrate into crystalline faces with lower energy. This results in the formation of smoother shapes. At high amounts of AsA or high pH, there is an abundance of Au0 creating a very high supersaturation and the formed Au0 can integrate readily with the seeds. Under these conditions, the formation of Au0 is much faster than the integration into the crystal, leading to rough growth.
Extending our mechanism to understand the shapes obtained, we observe that at lower supersaturation, the driving force is less and structures like NRs are formed. These have a smoother surface and well-defined edges. At high supersaturation, rougher NPs like ERs are obtained and at even higher supersaturation values (high pH with OA) an abundance of Au0 around the seeds leads to sphere-like shapes. The abundance of Au0 is believed to trigger a second nucleation phase, which can lead to higher kinetics and smaller sizes. This can be observed in the first order k values determined using our UV-Vis methodology that show an increase by one order of magnitude between NRs and sphere-like structures. In the experiments where the driving force increases, an increase in the first-order rate constant is always observed. This is in synchrony with concepts borrowed from classical crystallization theory where the kinetics of crystal growth depends on the supersaturation and increases as the supersaturation increases. The growth kinetics and shape dependency of NPs on supersaturation can also be extended to the double seeded method, in which case, at low supersaturation, smooth and well-defined tetrahexahedral structures are obtained and at high supersaturation, multifaceted spheres are obtained. This characteristic behaviour between growth and the driving force (supersaturation) can be summarized as follows. Smooth growth occurs at a lower driving force leading to the formation of NRs and THHs while rough growth contributes to the formation of ERs, NMs, spheres, multifaceted spheres, etc. These types of growth and crystal structures are in agreement with the classical crystal growth mechanism that describes the effect of supersaturation as a driving force that leads to the formation of smooth and rough structures at low and high supersaturation, respectively. The formation of NRs and THHs is similar to the formation of polyhedral structures; on the other hand, the formation of ERs and sphere-like structures is similar to dendritic and spherulite growth. Thus, by employing an understanding from classical nucleation theory, we believe that our approach will provide further mechanistic insights into the growth of Au NPs in a seeded growth approach employing binary surfactant mixtures.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0na00214c |
‡ These authors contributed equally. |
This journal is © The Royal Society of Chemistry 2020 |