aBiomaterials Group, School of Metallurgy and Materials, University of Birmingham, Edgbaston, Birmingham, B15 2TT, UK. E-mail: a.stamboulis@bham.ac.uk
bSchool of Engineering and Innovation, The Open University, Walton Hall, Milton Keynes, MK7 6AA, UK
cSchool of Pharmacy, University of Nottingham, Nottingham NG7 2RD, UK
First published on 6th May 2020
The surface of a medical implant is required to interact favourably with ions, biomolecules and cells in vivo, commonly resulting in the formation of the extracellular matrix. Medical grade Ti6Al4V alloy is widely used in orthopaedic and dental applications for bone replacement due to its advantageous mechanical properties and biocompatibility, which enhances the adhesion between native tissue and the implanted material. In this study, chemical and thermal modification of a medical-grade Ti6Al4V alloy were performed to enhance electrostatic interactions at the alloy surface with a synthetic peptide, suitable for conferring drug release capabilities and antimicrobial properties. The modified surfaces exhibited a range of topographies and chemical compositions depending primarily on the treatment temperature. The surface wetting behaviour was found to be pH-dependent, as were the adhesive properties, evidenced by chemical force titration atomic force microscopy.
The surface topography and charge density of Ti and its alloys are properties that can be modified by chemical treatments.7,12–14 One approach to alter these surfaces chemically is to use H2O2 in aqueous solution. This modification produces a titania gel layer (TGL) rich in OH− with nano and microporosity8,15 which is desirable for the adsorption of ions, peptides, and proteins, as well as the promotion of cell adhesion.16–18 Furthermore, the TGL on the surface can protect the supporting metal from corrosion in the biological environment.7,18 This is particularly relevant to the use of titanium for implantation. This chemical treatment, combined with a thermal treatment, form a TiOx surface that can prevent the liberation of cytotoxic elements from the bulk titanium into the surrounding tissues. This is supported by Browne and Gregson, who found that the release of titanium and aluminium ions from the oxide films on Ti6Al4V annealed at 400 °C for 0.75 h was reduced from 0.14 to 0.03 μg cm−2 (Ti), and from 0.25 to 0.026 (Al) μg cm−2, respectively, compared with the standard nitric-acid passivated surface.19 Control over the chemical moieties, charge density, and topography of the surface can be utilised for a multitude of applications. For example, rough surfaces can lead to the formation and deposition of calcium phosphates. The latter intervenes as anchorage for collagenous fibres produced by bone cells or osteoblasts, and in most of the cases helps to introduce biocompatibility.20
A previous study reported that a Ti6Al4V surface treated by H2O2 exhibited improved electrostatic adsorption of peptides;21 however, the surface properties were not reported. This study aims to show how the thermal oxidation and chemical treatment with H2O2 of a medical-grade Ti6Al4V surface can affect its chemical composition and topography in the view of the surface capability to interact with organic molecules such as peptides for drug delivery applications and antimicrobial properties.
Ti6Al4V sample treatment | Abbreviation |
---|---|
Polished surfaces | MPT |
Thermally oxidised | TO |
Chemically treated | TGL |
Thermally treated | TOn (n = 500, 600, 700 and/or 800 °C) |
Chemically and thermally treated | TGL-TOn (n = 500, 600, 700 and/or 800 °C) |
The vertical deflection and z-axis displacement data were recorded at a frequency of 10 kHz. A grid of 100 force-displacement curves was acquired for each sample/liquid combination, equally spaced over an area of 100 μm × 100 μm. The force-displacement data were analysed using JPK Data Processing software (JPK Instruments, UK).
A schematic of the measured forces is shown in Fig. 1. The out-of-contact repulsion force (Frep) was measured in the first peak from right to left of the approaching curve, the height of the triangle that was formed in the peak from the origin to the highest part of the peak until the signal was stable in the approach curve was measured as the force. The jump to force (FJT) was measured in the minimum point of the approach curve, and the pull-off force (FPO) was measured in the minimum point of the retract curve.
Peaks in the survey spectra were assigned using the Scofield library, and a linear background was used for all peaks. Deconvolution of the Ti 2p peaks obtained from the high-resolution scans was performed according to the literature24,25 applying two adjacent regions ranging from 451.79 eV to 461.5 eV and 461.5 to 468.0, respectively. For both regions, a Shirley background with an average width of 2 was used, and the position at 461.5 eV was offset by a factor of 18. 8 components relating to the four oxidation states of Ti (0, II, III and IV) and the doublets for the 2p1/2 and 2p3/4 states expected for each of these four peaks were fitted in all spectra. For the untreated Ti6Al4V surfaces, the positions of all peaks except the two prominent Ti(IV) and the Ti(0) 2p3/2 peaks were constrained according to literature values.24,25 The Ti(0) 2p1/2 peak was restrained to +6.1 eV from the Ti(0) 2p1/2 peak. For all other samples, only the two Ti(IV) peaks were not constrained, all other position constraints were kept constant. ESI Table 1 shows a summary of all constraints used for the treated surfaces.†
Sample | AFM | |
---|---|---|
S a (nm) | S q (nm) | |
MPT | 0.7 | 2.1 |
TO500°C | 2.3 | 3.1 |
TO600°C | 10.2 | 15.2 |
TO700°C | 20.6 | 30.9 |
TO800°C | 106.9 | 133.5 |
TGL | 8.5 | 17.0 |
TGL-TO500°C | 12.0 | 26.7 |
TGL-TO600°C | 16.8 | 28.2 |
TGL-TO700°C | 49.0 | 69.2 |
TGL-TO800°C | 121.0 | 151.4 |
Fig. 4 XRD diffractograms for MPT and TO Ti6Al4V modified surfaces, α-Ti (JCPDS no. 44-1294), β-Ti (JCPDS no. 44-1288), anatase (JCPDS no. 21-1272) and rutile (JCPDS no. 21-1276). |
Fig. 5 XRD diffractograms for TGL and TGL-TO Ti6Al4V modified surfaces, α Ti (JCPDS no. 44-1294), β Ti (JCPDS no. 44-1288), anatase (JCPDS no. 21-1272) and rutile (JCPDS no. 21-1276). |
The Raman spectra of anatase, rutile and samples with and without chemical treatment after thermal oxidation are shown in Fig. 6 and 7, respectively. Active vibrational modes of anatase in the spectrum are assigned to Eg at 140 cm−1, Eg at 196 cm−1, B1g at 395 cm−1, A1g at 515 cm−1, and Eg 639 cm−1.26 Active vibration modes of rutile are assigned to B1g at 142 cm−1, Eg at 447 cm−1, A1g at 610 cm−1, and E2g 812 cm−1.27 The vibrational modes of Ti–O bonds were associated with the vibrational modes of anatase for the heat treatments at 500 and 600 °C and associated with rutile for the heat treatments at 700 and 800 °C for all Ti6Al4V modified surfaces.
Sample | Ti 2p % | O 1s % | V 2p % | Al 2s % | C 1s % | N 1s % | aOther% |
---|---|---|---|---|---|---|---|
a Other includes Ca, P, S and Si. | |||||||
MPT | 22.0 ± 0.7 | 52.3 ± 0.5 | 0.2 ± 0.0 | 4.2 ± 0.1 | 19.7 ± 0.9 | 0.7 ± 0.1 | 0.9 ± 0.1 |
TO500°C | 20.4 ± 0.1 | 52.5 ± 0.2 | 0.4 ± 0.0 | 3.8 ± 0.1 | 20.0 ± 0.3 | 1.1 ± 0.0 | 1.8 ± 0.1 |
TO600°C | 18.7 ± 0.8 | 53.3 ± 0.4 | 1.0 ± 0.1 | 4.5 ± 0.1 | 19.5 ± 1.0 | 1.1 ± 0.1 | 2.0 ± 0.2 |
TO700°C | 15.4 ± 0.2 | 52.6 ± 0.4 | 2.4 ± 0.0 | 9.5 ± 0.1 | 18.6 ± 0.6 | 1.0 ± 0.1 | 0.5 ± 0.1 |
TO800°C | 11.3 ± 0.3 | 51.5 ± 0.6 | 2.3 ± 0.0 | 18.9 ± 0.3 | 15.3 ± 1.2 | 0.6 ± 0.0 | 0.1 ± 0.0 |
TGL | 19.2 ± 0.5 | 51.5 ± 0.3 | 0.2 ± 0.0 | 3.6 ± 0.1 | 22.3 ± 0.9 | 1.3 ± 0.1 | 1.9 ± 0.1 |
TGL-TO500°C | 15.4 ± 1.9 | 51.1 ± 3.6 | 1.5 ± 0.1 | 9.7 ± 0.7 | 20.7 ± 5.6 | 1.3 ± 0.6 | 0.2 ± 0.0 |
TGL-TO600°C | 13.1 ± 0.1 | 52.8 ± 0.8 | 3.0 ± 0.0 | 12.5 ± 0.2 | 17.3 ± 1.0 | 1.1 ± 0.1 | 0.1 ± 0.0 |
TGL-TO700°C | 12.2 ± 0.1 | 52.6 ± 1.2 | 3.2 ± 0.1 | 14.4 ± 0.3 | 16.4 ± 1.5 | 1.0 ± 0.1 | 0.2 ± 0.1 |
TGL-TO800°C | 6.5 ± 0.6 | 49.9 ± 1.5 | 2.0 ± 0.1 | 26.9 ± 0.2 | 14.0 ± 2.4 | 0.6 ± 0.1 | 0.2 ± 0.0 |
The high-resolution Ti 2p spectra of the Ti6Al4V modified surfaces (Fig. 8) are used for the curve fitting to determine the relative amounts of the four oxidation states of Ti present on the surfaces. The percentage contribution of each Ti oxidation state of the MPT Ti6Al4V modified surface is shown in Table 4. In all spectra, the predominant oxidation state was Ti(IV). Only the MPT Ti6Al4V modified surface displayed a notable second component for Ti(0). Ti(III) was also detectable in small amounts on all samples. Ti(II) and Ti(0) (with the exception of the MPT Ti6Al4V modified surface) were not present in any notable quantities.
Sample | Ti(0) % | Ti(II) % | Ti(III) % | Ti(IV) % |
---|---|---|---|---|
MPT | 11.1 ± 02 | 2.5 ± 0.1 | 11.8 ± 0.3 | 74.6 ± 0.5 |
TO500°C | 0.4 ± 02 | 0.6 ± 0.0 | 5.7 ± 0.2 | 93.3 ± 0.1 |
TO600°C | 0.4 ± 0.2 | 0.6 ± 0.1 | 5.4 ± 0.1 | 93.5 ± 0.2 |
TO700°C | 0.4 ± 0.5 | 0.6 ± 0.6 | 5.4 ± 1.6 | 93.7 ± 0.9 |
TO800°C | 0.1 ± 0.1 | 0.0 ± 0.0 | 9.8 ± 1.0 | 90.1 ± 0.9 |
TGL | 0.7 ± 0.2 | 0.5 ± 0.1 | 6.5 ± 0.2 | 92.4 ± 0.3 |
TGL-TO500°C | 0.0 ± 0.0 | 0.9 ± 0.2 | 5.7 ± 0.1 | 93.5 ± 0.2 |
TGL-TO600°C | 0.0 ± 0.0 | 0.0 ± 0.0 | 8.7 ± 0.8 | 91.3 ± 0.8 |
TGL-TO700°C | 0.1 ± 0.1 | 0.5 ± 0.8 | 7.0 ± 2.5 | 92.4 ± 1.6 |
TGL-TO800°C | 1.4 ± 1.0 | 0.0 ± 0.0 | 7.4 ± 0.4 | 91.2 ± 1.0 |
Fig. 9 Measurements of (a) θa, (b) Frep, (c) FJT and (d) FPO force distance curves of MPT Ti6Al4V modified surface in the presence of acidic and alkaline solutions at pH 3, 5, 7 and 9. |
The force–distance data obtained by AFM performed against the MPT surface at pH 3, 5, 7 and 9 are shown in Fig. 9b–d. The Frep increased with increasing pH, the FJT was higher when pH was acidic compared to the other solutions pH, and the FPO decreased at pH 9 compared with pH 3, 5 and 7.
The θa of the TGL and TGL-TO500°C surfaces are shown in Fig. 10, in which the TGL-TO500°C surface exhibited a higher θa than the TGL surface. Furthermore, the TGL surface exhibited a lower θa at pH 5–9 (θa ∼ 15°) than at pH 3 (θa ∼ 20°), whereas the TGL-TO500°C surface did not respond as strongly to pH change, exhibiting a minimum θa of 33° at pH 3, and a maximum θa of 38° at pH 7.
On the other hand, the chemically treated surface before thermal oxidation showed pores formation, the number of which increased with increasing the temperature of the TO process. A similar effect was reported by Wang et al.8 who suggested that porous TGL was formed on the surface of chemically treated (8.8 M H2O2/0.1 M HCl aqueous solution at 80 °C for 30 min) pure titanium (CP-Ti) after TO using temperatures in the range of 300–800 °C in air.
On the other hand, Raman spectroscopy (Fig. 6) confirmed that samples treated below 800 °C showed vibrational modes associated with both anatase and rutile crystal phases. In contrast, at 800 °C, the vibrational modes were associated only with rutile. These results are in agreement with Chang and Huang7 who studied the TiO2 crystal transformation by Raman spectroscopy. They reported that amorphous TiO2 and anatase were present in Ti6Al4V samples treated between 400 and 550 °C. Rutile formation began at 550 °C, whereas the metastable phase of anatase was transformed completely to rutile after heat treatment at 700 °C, suggesting that only rutile phase was formed at temperatures above 700 °C.
In contrast, the crystal characterization for chemically treated Ti6Al4V that underwent further treatment by TO at low temperatures did not show the presence of TiO2 crystal phases (Fig. 5). Kim et al.32 reported that the TGL obtained after treatment with NaOH and thermal treatment at 600 °C was amorphous. In our case, the broad lines at 24, 28 and 48° in the X-ray diffractogram (Fig. 5), as well as the broad Raman peaks at the vibrational modes of Ti–O bonds in the Raman spectra (Fig. 7), indicated that the oxide layer formed was indeed amorphous.
Chemical analysis of MPT surfaces confirmed the presence of Al, Ti, O, C and small amounts of V and N in the passive oxide layer. This was in accordance with the XPS study of Ti6Al4V surfaces performed by Roessler et al.2 and Milošev et al.33 who reported the presence of Al in the passive oxide as well as C, associated with adsorbed hydrocarbons. In our case, small traces of other elements (Ca, P, S and Si) were also detected on the MPT Ti6Al4V surfaces and are believed to be associated with residual elements from manufacturing not specified by the supplier.
High-resolution spectra of the Ti 2p peak showed that Ti (IV) is the main Ti oxide present (above 90%; Fig. 8 and Table 3). Some Ti (III) was detected on all samples, whereas Ti(II) and Ti(0) were only present in trace amounts. This indicates that the temperatures used here had little impact on the composition of the oxidation states of the surfaces. An exception of this is the untreated polished MPT surface that contained 11% Ti(0) and 11.8% Ti(III) and therefore a slightly lower relative amount of Ti(IV) (74.6%). This result was in accordance with the study performed by Lee and Chang34 on Ti6Al4V native surfaces who detected the same sub-oxides measured by XPS.
The Al and V content of the oxide layer was increased with increasing the treatment temperature, as is shown in Table 3. Du et al.35 reported that Al diffused from the substrate to the outer surface as Al2O3. Al diffusion was more pronounced with increasing the treatment temperature. Kumar et al.29 came to a similar conclusion, reporting that thermally treated Ti6Al4V surfaces were Al enriched compared with untreated Ti6Al4V. The V and Al enrichment were also reported by MacDonald et al.35 in surfaces thermally treated at 600 °C. In addition, C and N were observed to be present on the surface of thermally oxidised Ti6Al4V surfaces, as shown in Table 3. Still, their levels were considerably decreased when the temperature increased above 500 °C.
The increased O/Ti ratio for the TO treated sample at 500 °C (Table 3), with and without prior chemical treatment, compared with that of the untreated sample, was mainly due to O diffusion in the substrate and consequent formation of the oxide layer. The O/Ti ratio increase at treatment temperatures above 500 °C was due to the formation of a more dense oxide layer, in agreement with Guleryuz and Cimenoglu.28 They reported that dense oxide layers could be obtained at temperatures between 600–800 °C.
In addition, the XPS analysis of TGL-TO Ti6Al4V surfaces, also shown in Table 3, reveals that the Al content increased with increasing the treatment temperature, whereas the change in the V was very small. Sun and Wang36 reported that TGL formed on the Ti6Al4V surface might act as a diffusion barrier, preventing Al and V ions diffusing to the surface from the substrate. In our case, this might be true for V; however, it was obvious that the aluminium content increased consistently with increasing the treatment temperature for the TGL-TO Ti6Al4V.
In Fig. 9a, the θa of the MPT surface was highest at pH 5. This maximum could be associated with the isoelectric point (IEP) of the native titanium oxide (nTiOx), as explained by Chau and Porter.37 They reported that in the absence of specific absorbed ions, the maximum angle in the contact angle titration must be related to the IEP. This was also confirmed by McCafferty and Wightman40 who determined the IEP of Al2O3 and Cr2O3 as the maximum value obtained by contact angle titration. According to the literature, the IEP of TiOx occurs between pH 4–6.41 It has also been reported that the IEP of TiOx is influenced by the density of hydroxyl groups present in crystal phases, contamination, and inclusion of ions.2 For example, the IEP of anatase can vary between pH 5.9–6.6 and of rutile between pH 4.7–6.0.2 Moreover, Roessler et al.2 found that the surface IEP of native oxide on Ti6Al4V was around pH 4.4. Based on the information above, the use of contact angle titration is a suitable method for accurately determining the IEP of MPT surfaces only, considering that the high roughness of thermally and/or chemically treated samples interfered in the measurement and the data obtained was more suited to a qualitative assessment of surface charge.
The AFM adhesion study of MPT surfaces reinforced the argument that the IEP is around pH 5. The AFM adhesion analysis was performed with a Si cantilever that typically has a native SiO2 layer with an IEP reported in some studies between pH 1 and 4 (ref. 42–44) and in some other studies at pH 3.9.45,46 Raiteri et al.43 reported the dependence of SiO2 charge as a function of pH. The lowest Frep of MPT surface shown in Fig. 9b, and the highest attraction force shown in Fig. 9c, were observed at pH 3; this suggests that the cantilever was negatively charged and the MPT surface was positively charged. For solutions with pH > 5 it was expected that the negative charges of both SiO2 and the native TiOx layer formed on the MPT surface increased in magnitude. This was verified by the calculation of Frep, which increased with increasing pH (from pH 5) reaching the highest value at pH 9. Butt et al..47 also reported the Frep and attractive forces of a mica surface using an alumina probe. Frep was only detected when the pH was above 8.1, and attractive forces occurred below pH 8.1. This was because the mica surface was negatively charged at the pH measured by Butt (between pH 3.1 and 10.4) and the alumina probe IEP was 8.1.47
The FPO of the MPT surface, shown in Fig. 9a–d, exhibited their highest values at pH 5 and 7, yet a lower value at pH 9. These results can be explained considering that one of the surfaces was more negatively charged than the other, suggesting that the effect of the diffuse double-layer was involved in the interactions between the cantilever and the surface.48 Hence, the reduced negatively charged MPT surface (nTiOx) attracted water molecules than the negatively charged cantilever surface (SiO2). This allowed the forces in the aqueous interface to interact, generating larger adhesion forces at pH 5 and 7 compared with those at pH 9, where both surfaces were negatively charged. The reduction of the magnitude of the surface potential when the pH was closer to the IEP was reported by Walsh et al.48 They experimented on surfaces and a cantilever that were coated with TiO2 using atomic layer deposition (IEP at pH 5.1) and observed that the surfaces at pH 6.5 were negatively charged. Still, the charge was not as large as at pH 10, where the diffuse double-layer was large enough to create repulsion between both surfaces.
The trend of the advancing contact angle with the increase of the thermal treatment is to decrease due to roughness and topography, as evidenced in Fig. 3. However, the contact angle of TGL-TO500°C surfaces was higher than that measured for TGL surfaces at all pH (Fig. 10), even when the thermally treated surface presented a higher average roughness (Sa) than TGL surfaces (Table 2). This was an unexpected result. It has been reported that chemical treatment with peroxide can introduce Ti-complexes such as Ti-superoxide, TiO2−, Ti-peroxide and TiO2.49–51 However, Osaka et al.52 reported that further heat treatment in the air would result in the elimination of these Ti-complexes, leading to reduced hydrophilicity; these chemical reactions have been described by Osaka et al.52 and Tengvall and Lundström.6 The Ti-complexes slowly form polynuclear cations and anions leading to the precipitation of peroxotitanium hydrates (Ti(IV)O3(H2O)x with x = 1, 2 or TiO3(aq)). The peroxotitanium hydrate species was suggested to form μ-bridges (Ti–O–Ti) and consist of Ti2O5.6,52 Osaka et al.52 detected the presence of –O–O– (related with the peroxotitanium hydrate species) on pure Ti treated with H2O2 samples by FT-IR at 890 cm−1. After the thermal treatment at 400 °C, the absence of the peak at 890 cm−1 in the FTIR spectra suggested that the additional thermal treatment eliminated the –O–O– groups. It is likely therefore that such an elimination of –O–O– groups might happen in the case of the TGL-TO500°C surface, and for that reason, the contact angle was larger than for the TGL samples that were not thermally treated.
All modified Ti6Al4V surfaces showed an increase in surface roughness with increasing the thermal treatment temperature. In addition, TGL-TO samples treated at low temperatures (500–600 °C) exhibited an etched surface originated from the H2O2 treatment performed prior to the thermal treatment, whereas the TGL-TO samples treated at high temperatures presented a topography surface due to the thermal oxidation. Amorphous TiO2 was predominantly present in the passive TiOx layer for all samples, but after heat treatments and with increasing the temperature, this layer became crystalline and predominantly rutile confirmed by both XRD and Raman spectroscopy.
Al and V diffusion from the substrate occurred in almost all thermally treated samples with Al content increasing with increasing the treatment temperature.
DCA analysis showed that the IEP of the MPT sample surface was around pH 5. In addition, AFM suggested that the surface was positively charged in aqueous solutions below pH 5, and negatively charged above pH 5. The FPO values measured for the MPT surface showed, that when a strong negatively charged cantilever was used, a reduction in magnitude, as well as increased adhesion forces, were observed when the pH was close to the IEP.
Finally, the thermal treatment of TGL samples at 500 °C influenced the surface wettability. This suggested that the elimination of Ti–H2O2 during the thermal treatment at 500 °C for the latter resulted in different surface composition and topography.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra11000c |
This journal is © The Royal Society of Chemistry 2020 |