Nguyen Tat Thanga,
Le Thi Honga,
Nguyen Hoang Thoanb,
Chu Manh Hung*a,
Nguyen Van Duy*a,
Nguyen Van Hieucd and
Nguyen Duc Hoaa
aInternational Training Institute for Materials Science (ITIMS), Hanoi University of Science and Technology (HUST), No. 1-Dai Co Viet Str., 100000 Hanoi, Vietnam. E-mail: mhchu@itims.edu.vn; hung.chumanh@hust.edu.vn; nguyenvanduy@itims.edu.vn; duy.nguyenvan@hust.edu.vn; Fax: +84 24 38692963; Tel: +84 24 38680787
bSchool of Engineering Physics, Hanoi University of Science and Technology (HUST), No. 1-Dai Co Viet Str., 100000 Hanoi, Vietnam
cFaculty of Electrical and Electronic Engineering, Phenikaa Institute for Advanced Study (PIAS), Phenikaa University, Yen Nghia, Ha-Dong District, 100000 Hanoi, Vietnam
dPhenikaa Research and Technology Institute (PRATI), A&A Green Phoenix Group, 167 Hoang Ngan, 100000 Hanoi, Vietnam
First published on 31st March 2020
Fabrication of a high-performance room-temperature (RT) gas sensor is important for the future integration of sensors into smart, portable and Internet-of-Things (IoT)-based devices. Herein, we developed a NO2 gas sensor based on ultrathin MoS2 nanoflowers with high sensitivity at RT. The MoS2 flower-like nanostructures were synthesised via a simple hydrothermal method with different growth times of 24, 36, 48, and 60 h. The synthesised MoS2 nanoflowers were subsequently characterised by scanning electron microscopy, X-ray diffraction, Raman spectroscopy, energy-dispersive X-ray spectroscopy and transmission electron microscopy. The petal-like nanosheets in pure MoS2 agglomerated to form a flower-like structure with Raman vibrational modes at 378 and 403 cm−1 and crystallisation in the hexagonal phase. The specific surface areas of the MoS2 grown at different times were measured by using the Brunauer–Emmett–Teller method. The largest specific surface area of 56.57 m2 g−1 was obtained for the MoS2 nanoflowers grown for 48 h. This sample also possessed the smallest activation energy of 0.08 eV. The gas-sensing characteristics of sensors based on the synthesised MoS2 nanostructures were investigated using oxidising and reducing gases, such as NO2, SO2, H2, CH4, CO and NH3, at different concentrations and at working temperatures ranging from RT to 150 °C. The sensor based on the MoS2 nanoflowers grown for 48 h showed a high gas response of 67.4% and high selectivity to 10 ppm NO2 at RT. This finding can be ascribed to the synergistic effects of largest specific surface area, smallest crystallite size and lowest activation energy of the MoS2-48 h sample among the samples. The sensors also exhibited a relative humidity-independent sensing characteristic at RT and a low detection limit of 84 ppb, thereby allowing their practical application to portable IoT-based devices.
Recently, transition metal dichalcogenides such as MoS2 have been considered as a good sensing layer for low-temperature gas sensors because of their high surface-to-volume ratio, distinct semiconducting behaviour, abundant reactive sites for redox reactions and high mobility at RT.9–12 Possessing a layered structure stacked by weak van der Waals interaction, MoS2 has been prepared with different nanostructures by various methods. For example, many groups reported the synthesis of monolayer, bilayer and few-layer MoS2 nanosheets and/or thin film by chemical vapour deposition.13–15 Using the same method, Kumar et al. synthesised nanostructures of vertically aligned MoS2 flakes and nanowire networks.16,17 A previous study also formed MoS2 nanoflakes through sonication-assisted exfoliation.9 Several 3D MoS2 nanostructures, such as spheres and nanosheets, were synthesised using a hydrothermal approach,18–20 which is a simple and low-cost mass-production synthesis method with growth parameters that can be easily controlled. Regarding the sensing characteristics of hydrothermally synthesised MoS2 nanostructures, Zhang et al. fabricated sensors based on MoS2 nanospheres grown via a hydrothermal procedure assisted with CTAB for NO2 detection.21 However, the sensors operate at a high temperature of 100 °C and exhibit a gas response of 60% to a high NO2 concentration of 50 ppm. The MoS2 nanosphere structure synthesised by Yu et al. shows a gas sensitivity of 78% to 50 ppm NO2 at a similarly high temperature of 150 °C.19 In these works, although the operating temperature (OT) of the sensors is lower than that of SMO-based sensors, the sensors work at about 100 °C or 150 °C, causing high power consumption. To further reduce the OT of sensors, Lee et al. fabricated sensors based on surface-activated MoS2 nanosheets with excess sulphur precursor. The sensors work at RT, but their response to a high NO2 concentration of 100 ppm is as low as 99.3%.20 Similarly, sensors based on PbS quantum dot/MoS2 composites show an optimal OT at RT but a low sensitivity of 22.5% to 100 ppm NO2.22 The gas-sensing performance of MoS2 materials is strongly dependent on material morphology and quality, such as specific surface area and crystallite size. Such parameters can be determined by the synthesis method. Thus, a controllable synthesis of MoS2 materials to develop high-performance RT sensors for low concentration of poisonous gases is required for the IoT-based practical application of gas sensors.
This study reported the controlled synthesis of pristine MoS2 nanoflowers with different growth times of 24, 36, 48 and 60 h by using a simple hydrothermal method that does not require further processes, such as surface functionalisation, decoration and/or doping. The synthesised MoS2 nanostructures having the largest specific surface area and the smallest crystallite size showed excellent gas-sensing characteristics at RT to low NO2 concentrations of 1–10 ppm. The gas response of the sensor based on the synthesised MoS2 to a low NO2 concentration of 10 ppm at RT was as high as 67.4%. The fabricated sensors showed a low detection limit (DL), good selectivity to interfering gases and humidity-independent sensing characteristics at RT, which are crucial for their practical application to portable IoT-based devices.
Fig. 1 Experiment procedure for the controlled hydrothermal synthesis of MoS2 nanoflowers and drop-casting fabrication of the MoS2 sensor. |
(1) |
(2) |
Fig. 2 SEM images of MoS2 nanoflowers synthesised at different growth times: (a and b) at 24 h, (c and d) at 36 h, (e and f) at 48 h, (g and h) at 60 h. |
Fig. 3(a) and (b) reveal the XRD patterns and Raman spectroscopy of the MoS2-24 h, -36h, -48h, and -60h samples to investigate the crystal structure properties of the synthesised MoS2 flower-like nanostructures with different growth times. Aside from the XRD pattern of the MoS2 grown for 24 h, those of the rest showed pronounced peaks located at 2θ = 13.76°, 33.36°, 39.87° and 59.40°, which are indexed to the (002), (100), (103) and (110) planes of the hexagonal phase of MoS2, respectively (JCPDS-37-1492).27 The data showed that the diffraction peaks became higher and sharper with prolonged growth time, indicating an improvement of the crystallinity and the formation of the well-stacked layered structure of the MoS2 flower-like nanostructure along the c-axis.28 The crystallite size of the MoS2 nanostructures synthesised with different growth times was calculated using the Scherrer formula:
(3) |
Fig. 3 (a) XRD patterns and (b) Raman spectra of MoS2 nanoflowers synthesised at different growth times. |
Resonant Raman (RR) spectroscopy with a laser wavelength of 633 nm was used to investigate the atomic vibrational modes of the MoS2 flower-like nanostructures grown at different times. Fig. 3(b) shows the Raman spectra of the MoS2 flower-like nanostructures grown for 24, 36, 48 and 60 h. All spectra revealed three Raman vibrational modes located at approximately 378, 403 and 452 cm−1. The first two peaks indexed as E12g and A1g arose from the in-plane and out-of-plane vibrational modes of the hexagonal MoS2 between Mo and S and S and S, respectively.29 The frequency difference between two active modes of all the samples, which is a fingerprint to estimate the thickness of the MoS2 nanosheets, was rather similar. Thus, changes in the nanosheet thickness of the MoS2 grown at different times were difficult to discern. The intensity of the A1g mode was much higher than that of the E12g peak, which can be attributed to the spectra in the resonant condition of the MoS2 flower-like nanostructures.30,31 Under this condition, the direct transition with the final electronic state at K point is associated with dz2 orbitals of the Mo atoms.30 These are aligned in the vibrational direction of S atoms (A1g mode), resulting in strong electron–phonon coupling along the direction of the A1g mode. Thus, the enhancement of the A1g peak intensity with respect to the E12g peak occurred under RR spectroscopic conditions.30 The third peak at 452 cm−1 in the RR spectra of the MoS2 nanostructures was associated with the second-order longitudinal acoustic phonons (2LA(M) mode) at the M point.
To further investigate the atomic structure of the MoS2 flower-like nanostructures, we performed TEM measurements on the synthesised samples using Tecnai G2 20S-TWIN/FEI TEM with a thermal LaB6 electron gun at 200 kV offering a point resolution of 0.24 nm and lattice resolution of 0.144 nm. The MoS2 nanoflower material for measurement was prepared by dissolving a small amount of MoS2 nanoflowers into the ethanol solvent. A small drop of the solution was put onto the TEM specimen (copper grid with carbon foil) by using a micro pipette. Fig. 4(a) and (b) reveal representative TEM images of the MoS2 nanoflower grown for 48 h. The low-magnification TEM image, as shown in Fig. 4(a), indicates that the flower-like nanostructures were composed of curved ultra-thin nanosheets. The width of the uneven sheets was about several hundred nanometres. The high-resolution TEM image of the MoS2 nanostructures (Fig. 4(b)) reveals that the lattice fringes of the MoS2 were also curved but still clearly visible, thereby confirming the formation of the well-defined crystal structure of MoS2. The lattice fringe spacing was 0.63 nm, which was assigned to the (002) crystal plane of the MoS2 flower-like nanostructures. This result is in agreement with previous results.32 The compositional properties of the synthesised MoS2 flower-like nanostructures were investigated using EDX. Fig. 4(c) exhibits a representative EDX spectrum of the MoS2 nanoflowers grown for 48 h. In the measured energy range, the Kα and Lβ fluorescence lines of S and Mo were very close, respectively. Thus, deconvolution of the broad peak in the energy ranging from 2 keV to 2.6 keV of the EDX spectrum was performed. The result clearly showed the presence of S and Mo in the spectrum, which were generated in the synthesised flower-like nanostructures.
The specific surface area, one of the key parameters responsible for the high gas-sensing performance of the synthesised nanostructures was measured using the BET method by N2 adsorption isotherm at the relative pressure (P/Po) range of 0.05–0.3. The N2 adsorption quantities of the synthesised MoS2 nanostructures under four growth times as a function of relative pressure are shown in the ESI [Fig. S2(a)–(d)].† The BET specific surface areas of the four samples were calculated, as shown in Fig. 4(d). The specific surface area of the synthesised MoS2 nanostructures increased from 14.97 m2 g−1 to 56.57 m2 g−1 with prolonged growth time from 24 h to 48 h, respectively. When the growth time was further prolonged to 60 h, the BET specific surface area of the synthesised MoS2 nanostructures was reduced to 40.72 m2 g−1. The highest specific surface area was reached at 48 h growth time. The results are consistent with the above-mentioned XRD data of the MoS2 nanostructures. For a detailed comparison, Fig. 4(e) represents the correlation between the crystallite size and the specific surface area of the MoS2 synthesised with different growth times of 24, 36, 48 and 60 h. The graph indicates a strong correlation between the two parameters. The smaller crystallite size resulted in the larger specific surface area of the synthesised MoS2, which is in agreement with the theoretical relation between the two parameters (SBET ∼ constant/D, where SBET is the specific surface area and D is the crystallite size).33 The data confirm the largest specific surface area and smallest crystallite size obtained for the MoS2 synthesised with a growth time of 48 h Thus, this sample was expected to show the highest gas response among the different samples. The optimal experiment condition wherein the largest specific surface area and smallest crystallite size of the sample were reached for the growth of MoS2 nanostructures plays an important role in the development of a high-performance gas sensor based on MoS2 nanostructures.25
Prior to the gas-sensing measurements of the sensors based on the MoS2 nanostructures grown at different growth times, the current (I)–voltage (V) characteristics of the sensors were acquired in air with an applied bias voltage from −5 V to 5 V and temperature ranging from RT to 150 °C (data not shown). The current increased with increasing temperature, thereby indicating the semiconducting characteristic of the synthesised MoS2 nanostructures. The interface between the sensing layer and the Pt electrode showed a non-ohmic contact possibly because of the formation of the homojunction of the MoS2 nanoflowers.
The sensing layer with smaller activation energy has been demonstrated showing higher gas sensitivity of the sensor.34,35 The activation energy (Ea) of the MoS2 flower-like nanostructures can be calculated through the temperature-dependent conductivity as expressed by the Arrhenius eqn (4) as follows:34
(4) |
Fig. 5 Arrhenius fit of the ln(I(A)) versus 1/T of the MoS2 nanostructures grown for 24, 36, 48 and 60 h. |
Fig. 6(a) exhibits the transient resistance of the sensor to 1–10 ppm NO2 on the basis of the MoS2 flower-like nanostructures grown for 48 h at RT, 50 °C, 100 °C and 150 °C. The data showed that the baseline resistance of the sensor based on the MoS2 nanoflowers decreased when the OT was increased from RT to 150 °C, indicating the semiconducting characteristics of the synthesised MoS2. When the sensor was exposed to NO2 as an oxidising gas, the sensor resistance decreased, thereby showing p-type semiconducting behaviour. Fig. 6(b) reveals the sensor response in percent as a function of NO2 concentration at different OTs. The response of the sensor increased with increasing NO2 gas concentration from 1 ppm to 10 ppm. High amount to gas molecules contributes to absorption, and reaction increases gas sensitivity. The sensor exhibited the highest performance at RT within the measured temperature range, which can be attributed to large various active sites for gas adsorption at RT.2 Namely, the number of defects such as S vacancies was significantly high in the MoS2 at RT. It was about 5% as reported elsewhere for an identical system.9 These defects serve as reactive sites with the target gas, thereby increasing gas response at RT.19 When the working temperature of the MoS2 sensor was increased, the number of defects decreased, which reduced the number of reactive sites. Thus, the gas response decreased at higher temperatures.
Normally, the defect-dominated process on the surface of MoS2 contributes to the significant response and recovery times because of the high adsorption energy of the target gas with the defects as reactive sites.36 Previous works reported that sensors based on pristine MoS2 of different nanostructures have incomplete recovery at RT possibly because of the high adsorption energy of NO2 on the MoS2 surface or the strong binding between NO2 and the reactive sites of MoS2.17,37 However, some other works indicated that in spite of slow rates of gas adsorption and desorption, the pristine MoS2-based sensors showed the complete recovery at RT to target gases.20,38–40 This characteristic can be attributed to several factors, such as high specific surface area, defective/strained surface and weak van der Waals binding between the target gas and the MoS2 surface.20,38,39 In addition, Ikram et al. indicated that the high specific surface area not only increases the response of the sensor but also plays an important role in fast response and recovery times.41 Thus, understanding the detailed mechanism for the complete recovery of the sensor is still under debate because of the combined effects of physi-, chemi-sorption, role of defects sites and transduction mechanism37. As shown in Fig. 6(a), despite its slow rates, the sensor based on MoS2-48 h MoS2 showed complete response and recovery to NO2 gas at RT. This result can be mainly attributed to the large specific surface areas and the defects on the MoS2 surface.
For quantitative analysis, the response and recovery times of the MoS2-48 h MoS2 sensor to 1–5 ppm NO2 (no calculation at 10 ppm NO2 because the recovery resistance curves were not measured completely at this concentration) were deduced from its transient resistance, as shown in Fig. 6(c) and (d), respectively. The data showed that the response time of the sensor working below 100 °C was not much different. A similar behaviour was also obtained for the recovery time of the sensor at low temperatures. While the sensors working at high temperatures of 100 °C and 150 °C showed evidently faster response and recovery times than that working at low temperatures. The response/recovery times to 5 ppm NO2 were about 125 s/485 s and 95 s/320 s at RT and 150 °C, respectively. The fast response/recovery times can be attributed to the thermal energy generated at high temperatures, which reduced the defects on the MoS2 surface and accelerated the desorption of the absorbed gas.
The transient resistance curves of the sensors based on MoS2 grown for 24, 36, and 60 h to 1–10 ppm NO2 gas at different temperatures are shown in Fig. S3, S4 and S5† (in complementary data), respectively. The data also indicated the p-type semiconducting characteristic of the synthesised MoS2 under different growth times. The gas responses of each sensor are summarised in Fig. S3–S5.† Fig. 6(e) presents a comparison of the NO2 gas responses of the sensors based on the MoS2 grown for 24, 36, 48 and 60 h at RT. Among the sensors, the sensor based on the MoS2-48 h sample had the highest response to 1–10 ppm NO2. The highest gas response at 10 ppm NO2 was 67.4%. The highest sensitivity can be attributed to the synergistic factors of the largest specific surface area, smallest crystallite size and lowest activation energy of the MoS2-48 h sample as presented above, thereby contributing to the improved sensitivity of the sensor. For all the measured sensors, high gas response was obtained for the low activation energy, small crystallite size and large specific surface area of the MoS2 sensing layer. Namely, the gas sensitivity gradually decreased for the sensors based on MoS2 nanostructures grown for 48, 60, 36 and 24 h, which is consistent with their reduced specific surface area (56.57, 40.72, 28.55 and 14.97 m2 g−1), increased activation energy (0.08, 0.11, 0.13 and 0.15 eV) and crystallite size (3.51, 3.67, 3.81 and 4.43 nm).
The gas-sensing characteristics of the MoS2 nanostructures can be explained by the Langmuir–Hinshelwood mechanism for chemical reaction of the tested gas with adsorbed oxygen molecules on the surface of the sensing layer, leading to change in the sensor's resistance.36,42,43 As shown in Fig. 7(a), when the p-type semiconducting MoS2 nanostructures were exposed to ambient air, oxygen molecules were adsorbed on the MoS2 surface and electrons were captured from the valence band of the MoS2 to form the oxygen ion species (O2−, O− and O2−) (eqn (5)–(8)) as follows:
O2(gas) → O2(ads), | (5) |
O2(ads) + e− → O2−, | (6) |
O2(ads) + 2e− → 2O−, | (7) |
O2(ads) + 4e− → 2O2−. | (8) |
However, the sensors were measured at low temperature from RT to 150 °C; thus, the oxygen ion O2− was dominant.44,45 The adsorption of oxygen molecules on the surface of the p-type MoS2 by trapped electrons from the valence band resulted in a hole accumulation layer and decreased baseline resistance. When the NO2 was injected into the sensing layer, as illustrated in Fig. 7(b), the oxidising gas extracted electrons, which reacted with the adsorbed oxygen followed by, eqn (9) and (10) thereby creating more holes into the valence band.46 Therefore, the sensor resistance decreased upon exposure to NO2 gas, as follows:19,46
NO2 + e− → NO2−, | (9) |
NO2 + O2− + 2e− → NO2− + 2O−, | (10) |
NO2− + VS++ → NO2 + h+. | (11) |
A large number of defects such as S vacancies (VS++) at RT can be found in pristine MoS2, and these defects serve as reactive sites for target gas adsorption.19,36 The interaction mechanism between NO2 gas molecules and S vacancies is shown in, eqn (9) and (11) which generated significant holes into the valence band, thereby highly increasing the gas response at RT. When the temperature was increased, the electron mobility increased but the number of electrons may not be increased significantly; inversely, the number of S vacancies decreased drastically. As a result, less holes were created, and the response decreased at high temperatures.
Recent works on NO2 sensors based on different MoS2 nanostructures are summarised in Table 1 in terms of OT, gas concentration and gas response. The sensors based on pure MoS2 nanostructures showed very low response to NO2 gas even at high concentrations (5–500 ppm) under RT and elevated OT. The gas response of the sensors was increased by the surface functionalisation and heterojunction formation of the MoS2 nanostructures with other noble metals and metal oxide/carbon nanotubes, respectively. However, the enhancement of the response was still negligible and the NO2 gas concentration was extremely high (50–100 ppm). For example, Deokar et al. reported that a sensor based on MoS2–carbon nanotube hybrids exhibits a response of 12.6% to 50 ppm NO2 at RT.47 In the present study, the pure MoS2 flower nanostructure-based sensor showed a high response of 67.4% to a low NO2 concentration of 10 ppm under similar OT at RT.
No. | Materials | OT (°C) | Concentration (ppm) | Responsea (%) | Ref. |
---|---|---|---|---|---|
a Response was calculated by ; or | |||||
1 | MoS2 nanowire network | 60 | 5 | 18.1 | 17 |
2 | MoS2 nanospheres | 100 | 50 | 60 | 21 |
3 | MoS2–Au thin film | RT | 2.5 | 30 | 55 |
4 | MoS2/Si heterojunctions | RT | 50 | 28.4 | 56 |
5 | MoS2 layer | RT | 100 | 10 | 57 |
6 | Nanostructure MoS2 | 75 | 50 | 17.5 | 58 |
7 | UV-assisted 2D MoS2 | RT | 10 | 27.5 | 59 |
8 | MoS2 hollow spheres | 150 | 500 | 88.3 | 50 |
9 | PbS/MoS2 composites | RT | 100 | 22.5 | 22 |
10 | MoS2 nanoflowers | RT | 10 | 67.4 | This work |
The NO2 gas response of the sensor based on MoS2 nanostructures was the highest at RT. Thus, investigating the effect of humidity on the sensor characteristics is necessary for future practical applications. We measured the response of the representative gas sensor based on the MoS2-48 h sample to 1 ppm NO2 at RT under changing relative humidity (RH) from 60% to 90%. The RH was controlled using a lab-made setup, including a humidifier connected with a humidity sensor, as shown in Fig. S1.† Humidity was created in the sensing measurement chamber through a humidifier, and moisture content was detected by a humidity sensor connected to the humidifier. This sensor helps control the on/off state of the humidifier upon the set values of the RH. Fig. 8(a) exhibits the sensor resistance upon exposure to 1 ppm NO2 gas at RT with different RHs. The baseline resistance of the sensor based on p-type MoS2 nanostructures increased with increasing RH from 60% to 80%. The possible reason is the humid ambience, wherein water molecules interacted with lattice sites and/or defects as active sites on the MoS2 surface. As a result, more electrons were generated on the sensing layer surface. However, the synthesised MoS2 shows p-type semiconducting behaviour with majority charge carriers of holes, thereby increasing the resistance of the sensor in humid ambience.48,49 The resistance of the sensors gradually decreased when the RH was further increased to 90%. This observation is a characteristic of p-type materials and in agreement with previous works.48,49 On the basis of eqn (2), the calculated gas response of the sensor slightly decreased when the RH was increased from 60% to 90%, as shown in Fig. S6(f).† This result can be attributed to the presence of water molecules in the humid ambience, which interact with lattice sites and/or defects on the MoS2 nanoflowers, thereby decreasing the number of active sites for the adsorption of the tested gas.41,50 The large number of water molecules at high RH ambience results in less active sites and reduced surface area, thereby decreasing the gas response.41,50 However, the reduction in the response is small because the water molecules on the MoS2 surface are already abundant at 60% RH. Thus, further increasing the RH to 90% contributes insignificantly to further decreasing the number of active sites on the MoS2 nanoflowers. This phenomenon causes the gas response to slightly decrease with increasing RH. Therefore, humidity has a low effect on the MoS2 nanoflower sensor at RT. This finding is important in developing a NO2 gas sensor working at RT for future integration into smart and/or portable devices.
Although the sensor resistance varies with different RHs, the calculated gas response of the sensor relying on eqn (1) indicated an insignificant change with four measured RHs. This result demonstrated the RH-independent sensing characteristics of the MoS2 flower-based sensors at RT, which play an important role in developing a NO2 gas sensor working at RT for future integration into smart and/or portable devices.
In addition to the humidity effect, the DL and selectivity of the fabricated sensor are also important parameters for practical applications. Fig. 8(b) and (c) display the fifth-order polynomial fit of 15 experimental data points and the linear fit of the gas response as a function of NO2 concentrations at RT, respectively. On the basis of the fitting results, the DL value of the fabricated sensor was calculated as follows (12):51
(12) |
(13) |
Fig. 8(d) displays the gas response of the sensor based on the MoS2-48 h sample to different oxidising and reducing gases (10 ppm NO2, 20 ppm SO2, 500 ppm NH3, 500 ppm CO, 1000 ppm H2 and 4000 ppm CH4) at RT for the analysis of the selectivity properties of the sensor. The transient resistance curves of the sensor upon exposure to different gases are shown in Fig. S6(a)–(e) in ESI.† Although the concentration of the interfering gases was much higher than that of NO2 gas, the sensitivity of the sensor to NO2 gas was still much higher than to the interfering gases. This result can be explained by the stronger electronic interaction of NO2 gas with MoS2 owing to the higher adsorption energy of NO2 on the active sites of the MoS2 nanoflowers compared with the other tested gases.16,17 This result is consistent with previous theoretical calculations on the adsorption energy of various gases on MoS2 materials.54 The sensors based on the MoS2-48 h sample have good selectivity.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra00121j |
This journal is © The Royal Society of Chemistry 2020 |