Srikanth Mateti,
Md Mokhlesur Rahman*,
Pavel Cizek and
Ying Chen*
Institute for Frontier Materials, Geelong Campus, Deakin University, Waurn Ponds, 3216, Victoria, Australia. E-mail: m.rahman@deakin.edu.au; ian.chen@deakin.edu.au
First published on 14th April 2020
A solvent-free, low-cost, high-yield and scalable single-step ball milling process is developed to construct 2D MoS2/graphene hybrid electrodes for lithium-ion batteries. Electron microscopy investigation reveals that the obtained hybrid electrodes consist of numerous nanosheets of MoS2 and graphene which are randomly distributed. The MoS2/graphene hybrid anodes exhibit excellent cycling stability with high reversible capacities (442 mA h g−1 for MoS2/graphene (40 h); 553 mA h g−1 for MoS2/graphene (20 h); 342 mA h g−1 for MoS2/graphene (10 h)) at a high current rate of 250 mA g−1 after 100 cycles, whereas the pristine MoS2 electrode shows huge capacity fading with a retention of 37 mA h g−1 at 250 mA g−1 current after 100 cycles. The incorporation of graphene into MoS2 has an extraordinary effect on its electrochemical performance. This work emphasises the importance of the construction of the 2D MoS2/graphene hybrid structure to prevent capacity fading issues with the MoS2 anode in lithium-ion batteries.
In general, a common problem in preparing MoS2 based electrodes is that most of the production methods produce small quantity (milligrams), which is drastically different from existing industrial processes. The materials production process is vital because, if the production technique could not be adopted by industry, it would not be possible to commercially implement the electrode materials no matter how wonderful they are. Herein, we develop a simple scalable ball-milling technique to produce a large quantity of MoS2/graphene hybrid nanosheet electrodes via an in situ generation of graphene and 2D MoS2 where bulk graphite and bulk MoS2 used as starting materials as presented in Fig. 1. The obtained structure of MoS2/graphene heterointerface is expected to enhance the electronic conductivity and store more Li+, thus results in better electrochemical properties. The electrochemical performance of the MoS2/graphene hybrid nanosheets is improved drastically over the single system of either MoS2 or graphite when used as an anode material in LIBs.
For electrochemical measurements, the anode electrode was prepared by making a homogenous slurry of active material, conductive carbon additive (Super P Li™) and binder (CMC) with a weight ratio of 80%:10%:10% in water solvent. The slurry was then uniformly applied onto clean pieces of copper (Cu) foil with an area of 1 × 1 cm2. The coated Cu foil was dried naturally for 10 min then in a vacuum oven at 90 °C overnight. The loading of the electrode was around 1–1.5 mg cm−2. The dried electrodes were then pressed with 5 tons of load to enhance the contact between material and copper foil. The electrochemical cells (CR2032 coin type cell) were assembled in argon-filled glove box (<0.1 ppm O2) with working electrode (active materials coated onto Cu foil), polypropylene film as a separator, and Li metal foil as counter electrode. 1 M LiPF6, a mixture of ethylene carbonate (EC)/dimethyl carbonate (DMC)/diethyl carbonate (DEC) (1:1:1) used as electrolyte. The cells were galvanostatically discharged–charged at 25 °C in the voltage range of 0.01–3.0 V at 250 mA g−1 current using a LAND battery testing system (Wuhan LAND Electronics Ltd., China). Cyclic voltammograms (CV) were recorded using an Ivium electrochemical workstation at a scan rate of 0.05 mV s−1.
Fig. 2 XRD patterns of commercial graphite, commercial MoS2 and ball milled MoS2-G (10 h), MoS2-G (20 h), and MoS2-G (40 h) samples. |
Fig. 3 demonstrates SEM images of the pristine MoS2 and graphite, and ball milled MoS2/graphene hybrid. A typical low magnification SEM images of the pristine MoS2 (Fig. 3(a)) and graphite (Fig. 3(b)) reveal that pristine MoS2 and graphite consists of numerous large flakes or sheets like morphology. A significant change in morphology is observed between pristine MoS2 and graphite, and MoS2/graphene hybrids. During ball milling, large flakes of both pristine MoS2 and graphite are reduced to small flakes and simultaneously mixed them randomly and form 2D MoS2/graphene hybrid nanosheets. A typical morphology of MoS2/graphene hybrids is depicted in Fig. 3(c–h). It is clearly observed that MoS2 and graphite components are compacted into dense aggregates, which is prospectively beneficial for gaining an attractive capacity and for improvement of packing of the active material in a practical battery electrode. However, the duration of ball milling has an impact in the surface area of the hybrids. The specific BET surface areas of the hybrids were measured by the N2 adsorption/desorption method. The MoS2-G (20 h) hybrid shows the height surface area of 6.0 m2 g−1, whereas it was 2.0 m2 g−1 for MoS2-G (10 h) and 4.0 m2 g−1 for MoS2-G (40 h) hybrids. The result of BET surface areas is well consistence with morphology of the hybrids. It is visualised that 10 h and 40 h ball milled samples exhibit denser aggregates than that of 20 h hybrid (compare Fig. 3(d, f and h)). The relatively large specific surface area offers large material/electrolyte contact area, promote electrolyte ion diffusion to the active sites with less resistance12 and tolerate the volume change.13 Hence, it is anticipated that MoS2-G (20 h) hybrid may deliver a high reversible capacity with a stable cycle life as compared to MoS2-G (10 h) and MoS2-G (40 h) hybrids.
Fig. 3 SEM images: (a) commercial MoS2, (b) commercial graphite, and (c–h) MoS2/graphene hybrid nanosheets of (c and d) MoS2-G (10 h), (e and f) MoS2-G (20 h), and (g and h) MoS2-G (40 h). |
TEM examination was further carried out to evaluate the structural analysis of the MoS2-G (20 h) sample. Bright-field imaging of the sample reveals small flake-like dense morphology (Fig. 4(a)). The corresponding selected area electron diffraction (SAED) pattern of the sample is also depicted in the Fig. 4(b). The SAED pattern consists of both components of MoS2 and graphene that can be referenced to the crystallographic directions of (100), (102), (103), and (104) for MoS2 and (002), (100), and (101) for graphene, respectively. Fig. 4(c) represents HRTEM image of the sample. The in situ generated graphenes are composed of few-layers with a d spacing of approximately 0.35 nm, where nanocrystal of MoS2 is also clearly visible with a d spacing of approximately 0.70 nm (002).
Fig. 4 TEM investigation of the MoS2-G (20 h) sample: (a) a bright-field TEM image, (b) corresponding SAED pattern, and (c) HRTEM image of the sample. |
The electrochemical performance of the MoS2/graphene hybrid nanosheets was examined using CR 2032 coin-type cells in the voltage range of 0.01–3.0 V. Fig. 5(a) demonstrates the comparison of cycling performance of all electrodes in an identical testing condition. The incorporation of graphene into MoS2 has an extraordinary effect on its electrochemical performance. All hybrid electrodes of MoS2/G exhibit excellent cycling stability with high reversible capacities of 442 mA h g−1 for MoS2-G (40 h), 553 mA h g−1 for MoS2-G (20 h), 342 mA h g−1 for MoS2-G (10 h) at 250 mA g−1 after 100 cycles, respectively. The achieved reversible capacities are almost 85% for MoS2-G (40 h), 98% for MoS2-G (20 h), and 97% for MoS2-G (10 h) electrodes after 100 cycles with respect to the 3rd cycle reversible capacities, respectively. A significant capacity fading is observed for the MoS2 electrode with a capacity retention of 37 mA h g−1 at 250 mA g−1 after 100 cycles. Such a huge improvement in cycling performance of the hybrid electrodes, particularly cycling stability, suggests that the incorporation of graphene into MoS2 crystals not only tremendously increases electronic conductivity (both interparticle and intra-particle conductivity) but also improves the ionic conductivities of the hybrid electrodes.14 However, it is interesting to note that ball milling duration in the hybrid preparation plays a critical role in their electrochemical performance. Clearly, the MoS2-G (20 h) electrode shows better electrochemical performance (in terms of capacity and stability) than that of MoS2-G (10 h) and MoS2-G (40 h) electrodes, which is related to the high surface area as well as structural integrity of the MoS2-G (20 h) electrode.
Corresponding galvanostatic charge–discharge of the MoS2-G (20 h) electrode is depicted in Fig. 5(b). Fig. 5(b) shows the first, 2nd, 10th, 50th and 100th cycle discharge–charge curves of the electrode obtained at 250 mA g−1 within the voltage range of 0.01–3.0 V. When the electrode is discharged to 0.01 V (lithiation) and charged to 3.0 V (de-lithiation), both voltage profile exhibits typical plateaus which are consistence with the CV curves. The MoS2-G (20 h) electrode also delivers commendable initial coulombic efficiency. At the first cycle, the MoS2-G (20 h) electrode exhibits discharge/charge capacities of 485/338 mA h g−1, corresponding to the initial coulombic efficiency of ∼70% (Fig. 5(c)). The coulombic efficiency of more than 99% after the first few cycles indicates high reversibility of the composite electrodes, leading to a stable cycling performance. The electrochemical impedance spectroscopy (EIS) of the electrodes was performed in the fresh cells at OCP (open circuit potential) state. Typical Nyquist plots recorded for all electrodes are presented in Fig. 5(d). All plots display one compressed semicircle in the high to medium frequency region and a sloped line in the low frequency region. The diameter of each semicircle is related to the charge transfer resistance, the smaller the diameter, the smaller the charge transfer resistance, and the higher the electronic conductivity.15,16 A comparison of the diameters of the semicircles indicates that the impedance of the MoS2/graphene hybrid electrodes is significantly lower than that of the graphite and MoS2 electrodes, respectively. The incorporation of graphene into MoS2 particles under ball milling significantly enhances the conductivity of the MoS2/graphene hybrid electrodes, leading to much easier charge transfer at the electrode/electrolyte interface and consequently decreases the overall internal resistance of the cells.
Fig. 6 shows the cyclic voltammograms of the MoS2-G (10 h), MoS2-G (20 h), MoS2-G (40 h), and MoS2 electrodes measured at a scan rate of 0.05 mV s−1 in the voltage range 0.01–3.0 V. During the first discharge, two cathodic peaks appear between 1.0–1.25 V and 0.5–0.9 V for the MoS2-G electrodes, which can be attributed to the conversion reaction of MoS2 + 4Li+ → Mo + 2Li2S and the change in the coordination of Mo with six S atoms from trigonal prism to octahedron by inserting Li ions into the MoS2 layers (i.e., formation of LixMoS2) (1.0–1.25 V).2 It is observed that the cathodic peaks appeared between 0.5–0.9 V comprises broad peak, which should be correlated with the formation of a SEI (solid electrolyte interface) film on the surface of the electrodes.17 In the subsequent discharge process, the cathodic peaks are quite different from the first discharge and peaks are shifted to higher voltages and two new broad peaks appeared at 1.0 and 1.8 V, corresponding to the voltage plateau with the formation of Li2S and the association of Li ions with Mo.18 In the anodic scans, the electrodes display two peaks at 1.7 and 2.3 V, which are corresponding to the oxidation of Mo metal to MoS2 (1.7 V), while the pronounced oxidation peak at 2.3 V is due to the formation of sulfur.19,20 The MoS2 bulk electrode (Fig. 6(d)) shows three sharp cathodic peaks at 1.87, 1.08, and 0.31 V. In the anodic process, the MoS2 electrode exhibits two peaks at 1.7 V and 2.3 V, corresponding to the oxidation of Mo metal to MoS2 and formation sulfur. However, a pair of cathodic/anodic peak at around 0.19/0.27 V is visualised for the MoS2-G electrodes, which is assigned to the insertion/extraction of Li ions into the layer of graphene.2
Fig. 6 Cyclic voltammograms measured at a scan rate of 0.05 mV s−1 in the voltage range 0.01–3.0 V: (a) MoS2-G (10 h), (b) MoS2-G (20 h), (c) MoS2-G (40 h), and (d) MoS2. |
The obtained preliminary results indicate that the structure of 2D MoS2/graphene electrode is beneficial to the full infiltration of the electrolyte, reducing the migrating distance of Li ions, facilitating Li-ions exchange across the heterointerface by maintaining a large effective contact area between the active materials, conductive additives, and the electrolyte. Most importantly, the 2D MoS2/graphene hybrid nanosheets structure is capable of tolerating volume variation of the electrodes during Li-ions extraction/insertion, enhancing Li-ions storage kinetics and structural stability. The obtained electrochemical performance of the 2D MoS2/graphene hybrid electrode is promising and comparable with those of the reported results21–29 as summarised in Table S1 (ESI).† It is expected that a more robust electrode architecture of MoS2/graphene hybrid nanosheets prepared by controlled parameters could be used as an effective negative electrode for more sustainable, cost-effective Na-ion and K-ion batteries and this is to be demonstrated in our future work.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra01503b |
This journal is © The Royal Society of Chemistry 2020 |