Xianbo Yuab,
Jie Suna,
Wenna Zhao*b,
Shihang Zhaoa,
Hongmei Chena,
Kai Taoa,
Yaoping Hua and
Lei Han*a
aState Key Laboratory Base of Novel Functional Materials and Preparation Science, School of Materials Science & Chemical Engineering, Ningbo University, Ningbo 315211, China. E-mail: hanlei@nbu.edu.cn
bKey Laboratory for Molecular Design and Nutrition Engineering of Ningbo, Ningbo Institute of Technology, Zhejiang University, Ningbo, Zhejiang 315100, China. E-mail: wnzhao@nit.zju.edu.cn
First published on 6th April 2020
Bismuth oxide (Bi2O3) with high specific capacity has emerged as a promising negative electrode material for supercapacitors (SCs). Herein, we propose a facile metal–organic framework (MOF) derived strategy to prepare Bi2O3 microrods with a carbon coat (Bi2O3@C). They exhibit ultrahigh specific capacity (1378 C g−1 at 0.5 A g−1) and excellent cycling stability (93% retention at 4000 cycles) when acting as negative electrode material for advanced asymmetric SCs. The assembled Bi2O3@C//CoNi-LDH asymmetric supercapacitor device exhibits a high energy density of 49 W h kg−1 at a power density of 807 W kg−1. The current Bi-MOF-derived strategy would provide valuable insights to prepare Bi-based inorganic nanomaterials for high-performance energy storage technologies and beyond.
Recently, bismuth oxide (Bi2O3) has been considered as a promising negative electrode material due to its cheaper, environmental friendliness, abundant resources and high theoretical specific capacities (1370 C g−1 at 1 A g−1).8,9 For instance, Qiu et al.10 synthesized ultrathin Bi2O3 nanowires by oxidative metal vapor transport deposition technique, which exhibited high specific capacity (576 C g−1 at 2 A g−1). Shinde et al.11 grew 3D Bi2O3 by fast chemical method at room temperature, which demonstrated a specific capacity of 447 C g−1 at current density of 2 A g−1. Liu et al.12 designed oxygen-deficient r-Bi2O3/graphene flexible electrode with high specific capacity of 1137 C g−1 at 1 mA cm−2. Nevertheless, Bi2O3 still has disadvantages for ASCs, such as its intrinsically poor electronic and ionic conductivities, the large volume expansion in charging–discharging process. Improved researches have illustrated that the carbon can be used as a buffer layer, which could effectively reduce the morphological change and protect the structure of electrode. The facile design and preparation strategy of Bi2O3/C composites remains a continuing research to adjust the morphological and electronic structures.13–16
Metal–organic frameworks (MOFs) as sacrificial templates to derive nanocarbons or metal compounds/composites are an effective approach to obtain excellent electrode materials with high reversible capacity and cycle performance.17 Nano- or micro-structural metal oxides, carbides, phosphides and chalcogenides derived from MOFs have been extensively studied. Especially, the direct formation of carbon-doped composites can improve the conductivity and stability, which can ensure the rapid transfer of electrons.18 Ma et al.19 reported the MOF-derived hybrid Co3O4/C porous nanowire arrays. To our best knowledge, the fabrication of hybrid Bi2O3/C derived from Bi-based MOFs has not been reported.20
Herein for the first time, we report a Bi2O3@C microrod through a facile one-step heat treatment, using Bi-based MOF (CAU-17) as both template and precursor. Benefiting from the carbon coated layer from the pyrolysis of CAU-17, it can increase the electrical conductivity and ease the volume collapse during the discharge–charge process. The obtained Bi2O3@C hybrid as negative electrode for SCs exhibits ultrahigh specific capacity (1378 C g−1 at 0.5 A g−1) and excellent cycling stability (93% retention at 4000 cycles). In addition, ASC device using a layered double hydroxide (CoNi-LDH) as positive electrode provides a high energy density of 49 W h kg−1 at a power density of 807 W kg−1.
The specific capacity (Qs, C g−1) were calculated by the following equation:
(1) |
Before assembling an asymmetric supercapacitor, the load mass of the two working electrodes is balanced by the relationship of charge q+ = q−. The energy density (E) and power density (P) are calculated based on the total mass of the active materials of the two electrodes, according to the following equations:
C = Qs/ΔV | (2) |
(3) |
(4) |
Fig. 1 (a) XRD pattern of Bi2O3@C; (b) EDS spectrum of Bi2O3@C; (c–f) XPS spectra spectrum of Bi2O3@C: (c) survey spectra, (d) Bi 4f, (e) O 1s and (f) C 1s peaks. |
XPS test is further carried out to analyse the chemical compositions and detailed surface electronic states. The survey spectrum displays that the existence of Bi, C and O elements in as-prepared materials (Fig. 1c), which are in good match with the EDS results. As shown in Fig. 1d, the spin splitting of Bi 4f peaks consists of Bi 4f7/2 and Bi 4f5/2, located at 158.8 and 164.1 eV, respectively. Moreover, the peaks can be divided into four peaks, containing two kinds of oxidation states. The higher binding energy peaks of Bi3+ are attributed to 159.1 and 164.4 eV, whereas the peaks at 158.7 and 164.0 eV should be designated to Bi2+.25 Fig. 1e shows the O 1s spectrum, the peaks at 529.8 and 530.0 eV correspond to Bi–O and Bi–O–C bonds, 531.1 and 532.9 eV are attributed to the adsorbed water, respectively.26 The C 1s profile (Fig. 1f) indicates that the highly intensive peak (∼284.9 eV) can be assigned to sp2 hybridized carbon atoms, the other peak at ∼284.4 eV, ∼285.5 eV, and ∼288.7 eV are associated with C–O, CO, and O–CO, respectively.9
The morphology of CAU-17 presents hexagonal microrods (Fig. 2a). SEM image (Fig. 2b) of Bi2O3@C shows that the microrod morphology remains intact after the pyrolysis, while the hexagonal configuration is damaged. The smooth surface indicates that Bi2O3 is well encapsulated within the carbon layer. Benefiting from the periodic arrangement of organic motifs and metal nodes in Bi-MOF structure, the carbon formed in situ is uniformly coated on the surface of Bi2O3. Such unique hybrid structure may improve the conductivity and stability, which are beneficial for energy storage. The average diameter and length of Bi2O3@C microrods are about 820 nm and 3 μm, respectively, which are smaller than CAU-17 precursor (∼1.0 μm and ∼3.5 μm). This size shrinkage could be associated with the massive loss of organic components during the annealing process.27 TEM result (Fig. 2c) displays that Bi2O3@C is dense structure without pores. Furthermore, HRTEM image (Fig. 2d) exhibits the carbon was coated on surface of Bi2O3. The interplanar spacing between two adjacent lattice fringes is 0.302 nm, which is corresponding to (012) plane of Bi2O3. Additionally, SAED pattern present a good crystallinity of Bi2O3. Elemental mappings of an individual Bi2O3@C microrod indicate all elements are uniformly distributed in the whole structure (Fig. 2e–h).
Fig. 2 (a) SEM image of CAU-17; (b) SEM, (c) TEM and (d) HRTEM images of Bi2O3@C; (e–h) The elemental mappings of Bi, O, C and overlay. |
The electrochemical performances of Bi2O3@C as negative electrode are evaluated by CV and GCD measurements in 1 M KOH aqueous electrolyte. The CV cures (Fig. 3a) at different scan rates show a reversible charge–discharge response, and the distinct anodic and cathodic peaks are corresponding to the redox reactions of Bi0+, Bi2+ and Bi3+. The possible faradaic reaction mechanism is described as the following equation:9 Bi2O3 + 3H2O +6e− ↔ 2Bi + 6OH−. Also, the current densities of redox peaks increase with the increased scan rates, indicating fast redox reactions at the electrode/electrolyte interface. The GCD curves of Bi2O3@C electrode at different current densities (0.5–5 A g−1) are revealed in Fig. 3b, the observed plateaus at ∼−0.60 V and ∼−0.55 V, demonstrating the battery-like behaviour and excellent energy storage characteristics. In addition, the specific capacity calculated from GCD tests at different current densities is present in Fig. 3c. The Bi2O3@C electrode exhibits remarkable specific capacity, which are 1378, 1095, 937, 818 and 575 C g−1 at 0.5, 1, 2, 3 and 5 A g−1 respectively. The considerable specific capacity is superior to some previously related materials, such as AC (activated carbon)–Bi2O3 electrode (333 C g−1 at 1 A g−1),28 CQD (carbon quantum dot)–Bi2O3 (343 C g−1 at 0.5 A g−1),29 mesoporous 3-D Bi2O3 (447 C g−1 at 2 A g−1),11 Bi2O3 nanowires (576 C g−1 at 2 A g−1),10 and so on (Table S1†). Moreover, Bi2O3@C exhibits a remarkable cycling stability. As shown in Fig. 3d, the curve begins to rise gradually, attributing to the activation of electrode. With the increase of cycle number, it finally becomes stable, and remains 93% of the initial capacity at 5 A g−1 after 4000 cycles. These superior electrochemical performances of Bi2O3@C might be attributed to the following reasons. Firstly, the regular structure of CAU-17 could lead to the uniform distribution of the metal components and carbon in Bi2O3@C microrod, which improves the active surface area and effective electron transport during the electrochemical process. Secondly, the carbon-coated layer could enhance the electrical conductivity and the stability of Bi2O3@C.30
In addition, the charge storage mechanism for Bi2O3@C electrode is explored by low scan rate of CV, as shown in Fig. 3e. According to the Power law: i = avb, where i is the current (A), v is the scan rate (V s−1), a is constant and b is the Power law exponent. The value of b is calculated from the slope of logi vs. logν at a constant potential of redox, where b = 1 indicates capacitive-controlled mechanism and b = 0.5 is characteristic of diffusion-controlled mechanism.31 The obtained b value of Bi2O3@C is 0.53 indicates the diffusion charge storage is dominated. The fraction of diffusive charge storage fd is determined using the formula: fd = (1 − b)/0.5, which is used to calculate the capacitive and diffusive contributions of current.25 The value of diffusive charge storage is 0.94 for Bi2O3@C, further demonstrating the diffusion-controlled contribution. There is also a part of the capacitive-controlled contribution, which is caused by the carbon in hybrid Bi2O3@C. The EIS technique is also employed at the open-circuit potential in the frequency range from 100 kHz to 0.01 Hz. The Nyquist plots of Bi2O3@C electrode in Fig. 3f show a small line at low-frequency region and a semicircle at high-frequency region. The internal resistance (Rs) is equal to the intercept on the X-axis (1.68 Ω), the charge-transfer resistance (Rct) corresponds to the diameter of the semicircular loop at the high frequency (0.22 Ω). Moreover, the line with large slope is named Warburg resistance in the low frequency region, suggesting Bi2O3@C has excellent ion diffusion and fast charge transport speed.
To further investigate the practical application of hybrid Bi2O3@C electrode, an asymmetric supercapacitor (ASC) device is assembled in 1 M KOH electrolyte by employing Bi2O3@C/NF (nickel foam) and layered double hydroxide (CoNi-LDH/NF) as negative and positive electrode, respectively. The CoNi-LDH nanoflowers composed of ultrathin nanosheets are prepared through a typical method.20,32 The SEM and electrochemical properties of CoNi-LDH are displayed in Fig. S3.† The specific capacities of CoNi-LDH are 566, 544, 517, 459 and 354C g−1 at 1, 2, 3, 5 and 8 A g−1. The CV curves of ASC device are shown in Fig. 4a, the redox reaction peaks are revealed to different scanning rates (2–20 mV s−1) at the voltage range of 0–1.6 V, suggesting fast charge–discharge properties of the ASC device. The GCD curves of ASC device are shown in Fig. 4b. The specific capacity is excellent at voltage plateaus from 0 to 1.6 V, achieved 219 C g−1 at the current density of 1 A g−1. Ragone plots (energy density vs. power density) of ASC device is depicted in Fig. 4c. The energy density of Bi2O3@C//CoNi-LDH device is 49 W h kg−1 at a power density of 807 W kg−1, and still maintains 9 W h kg−1 at a high power density of 4050 W kg−1, which are advantageous over many previously reported ASC, such as AC//Bi2O3@C (18.94 W h kg−1, 1267 W kg−1),33 ESCNF@Bi2O3//CF@NiCo2O4 (25 W h kg−1, 786 W kg−1),34 Bi2O3//MnO2 (9.1 W h kg−1, 3370 W kg−1),35 Bi2O3–Ni–F//graphite (11 W h kg−1, 720 W kg−1)36 CoNi-LDH//AC (20.38 W h kg−1, 800 W kg−1).37 The capacity retention of Bi2O3@C//CoNi-LDH ASC is shown in Fig. 4d. It is noted that the cycling performance is unchanged at initial 2000 cycles, and still retains 81% of the initial capacity after 4000 cycles at a current density of 5 A g−1, suggesting a favorable stability of this ASC device. These results confirm that as-prepared Bi2O3@C is expected to be a potential candidate as negative electrode material and satisfy requirements of high-performance ASC device.
Fig. 4 Bi2O3@C//CoNi-LDH ASC device: (a) comparison of CV curves at different scan rates; (b) GCD curves at different current densities; (c) Ragone plots; (d) cycling performance. |
Footnote |
† Electronic supplementary information (ESI) available: Experimental and images of XRD, FT-IR, TGA, SEM, CV, GCD, and table. See DOI: 10.1039/d0ra01470b |