Open Access Article
This Open Access Article is licensed under a Creative Commons Attribution-Non Commercial 3.0 Unported Licence

Rapid synthesis of diol homolog-based thermosets with tunable properties via ring-opening metathesis polymerization

Liuyang Zhang , Fei Huangfu , Wanrong Li and Po Yang *
College of Polymer Science and Engineering, Sichuan University, State Key Laboratory of Polymer Materials Engineering, Chengdu, Sichuan 610065, China. E-mail: yangpo@scu.edu.cn

Received 10th March 2021 , Accepted 12th April 2021

First published on 12th April 2021


Abstract

This work aims to convert diols into thermosets with tunable properties. A series of diol-derived monomers have been synthesized and characterized. After mixing with second-generation Grubbs’ catalyst, these liquid monomers polymerize completely in two minutes to form cross-linked structures, which benefits rapid manufacture of composites. These diol homolog-based thermosets have good thermal properties and mechanical properties, and their performance can be greatly enhanced by fabricating woven flax fiber composites. We believe these may help researchers design and explore novel promising sustainable diol-based polymers and materials with excellent properties.


Introduction

Thermosets, e.g., (for instance, phenolic resins, epoxy resins, and benzoxazines) have attracted extensive interest in scientific and industrial communities due to their fascinating properties like good thermal stability and chemical resistance.1–3 Nevertheless, some disadvantages such as brittleness and tedious polymerization process limit their application. Obviously, more thermosets with tunable properties are desirable and valuable.

On the other hand, bio-based polymers and materials have become increasingly popular.4–8 This is due to the intensified environmental awareness as well as the desire to substitute dwindling fossil resources with sustainable alternatives.9–12 A promising approach is to synthesize thermosets using sustainable or bio-based compounds (for instance, diols, isosorbide and furan) as feedstocks.13–15 α,ω-Diols (diols, for instance, ethylene glycol, 1,3-propanediol, 1,4-butanediol and 1,5-pentanediol) can be obtained from biomass by microbial fermentation, hydrolysis and hydrogenolysis.16–18 As an abundant source of biomass compounds, diols are used as feedstock for the synthesis of bio-based thermosets, like polyurethanes and epoxy resins.19–21 Synthesis of these thermosets, nonetheless, requires a lot of energy, which produces lots of CO2 and NOx due to the complex and tedious process.22 For example, diol-based epoxy resins need to be cured at 140 °C (1 h) and 180 °C (1 h),19 and polyurethane also takes several hours to cure.23,24 In addition, these thermosets in general do not perform well.25,26 Consequently, there is still much interest in converting diols to thermosets with less energy, reducing their cost and environmental impact and furthering their application.

Ring-opening metathesis polymerization (ROMP) is a remarkable tool to rapidly convert cyclic olefins into acyclic dienes resulting in the formation of polymeric materials.27 Owing to ROMP, numerous polymers and polymeric materials like biomedical functional materials, ion exchange membranes, photoresist and photoinitiated polymers have been synthesized easily.28–34 With the aid of frontal polymerization technique, ROMP was also applied for rapid manufacture of high-performance cross-linked polymers and materials.35 If diols were converted to cyclic olefins moiety-containing monomers, they can be used to generate polymers via ROMP, which benefit to reduce the energy and expand their applications.

This work hence attempts to synthesize diol homolog-based thermosets and prepare composites via ROMP. Because the driving force of ROMP is the release of strain in the ring structures, norbornene-functionalized monomers can polymerize quickly in the presence of Grubbs’ catalysts.36 For rapid synthesis of diol homolog-based thermosets, this contribution achieved a series of dinorbornenyl-diol-derived monomers from 5-norbornene-2-carboxylic acid and diols, namely, ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol and 1,10-decanediol. Thorough investigation showed that these monomers can convert into cross-linked polymers in two minutes via ROMP. Moreover, the monomers, dinorbornenyl-pentanediol and dinorbornenyl-decanediol based esters can also be applied to prepare composites rapidly using the vacuum-assisted resin-transfer mounding (VARTM) technique. According to the results, diol homolog-based thermosets exhibit good properties and are fit for rapid fabrication of composites, and we developed new diol-based thermosets. Detailed analysis and discussions are provided below.

Experimental

Materials

5-Norbornene-2-carboxylic acid (98%), ethylene glycol (99.5%), 1,3-propanediol (98%), 1,4-butanediol (99%), 1,5-pentanediol (98%), 1,6-hexanediol (98%), 1,7-heptanediol (98%), 1,8-octanediol (98%), 1,9-nonanediol (98%), 1,10-decanediol (98%), triethylamine (99%), oxalyl chloride (98%), 4-dimethylaminopyridine (DMAP, 99%), N-(3-dimethylamino-propyl)-N’-ethylcarbodiimide hydrochloride (EDCI, 97%), methylene chloride (DCM, 99.5%), N,N-dimethylformamide (DMF, 99.8%), and methanol (MeOH, 99.5%) were purchased from Adamas-beta. Second-generation Grubbs’ catalyst (GC2) was purchased from Sigma-Aldrich. Woven flax fiber was purchased from China Shaoxing linen manufacturer. Tributyl phosphite was purchased from Alfa Aesar. All the reagents were used as received.

Synthesis of diol-based monomers

Diol-based monomers were synthesized from 5-norbornene-2-carboxylic acid and diols (i.e., ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol and 1,10-decanediol). Detailed syntheses are provided in the ESI. The chemical structures of the monomers (NB2, NB3, NB4, NB5, NB6, NB7, NB8, NB9 and NB10) are listed in Fig. 1.
image file: d1ma00210d-f1.tif
Fig. 1 Synthesis of diol-based monomers and thermosets. (i) oxalyl chloride, DCM. (ii) diols, triethylamine. (iii) GC2, 180 °C, 2 minutes.

Polymerization of diol-based thermosets

Diol-based thermosets were synthesized from the corresponding monomers. The GC2 solution was freshly made as described previously in ref. 35 and then added to the monomers. After thoroughly mixing and rapidly transferring to the PTFE mold, the monomers were polymerized at 180 °C for 2 minutes.

Preparation of composites

This work used five sheets of dry woven flax fibers to prepare the composites through the vacuum-assisted resin-transfer moulding (VARTM) technique (Fig. S10, ESI). NB5 or NB10 was mixed with GC2/phosphite solution to obtain liquid resin as matrix for composites. A low vacuum (−0.95 MPa) was applied to infuse the resins and compact the layup for producing the composites. After that, the layup was moved into an air oven at 180 °C for 2 minutes.

Characterization

Fourier transform infrared (FTIR) spectra were obtained from a Nicolet-560 spectrometer in the range of 4000–400 cm−1 at a resolution of 4 cm−1. 1H and 13C NMR spectra were recorded on a Bruker TD-65536 NMR (400 MHz) spectrometer using CDCl3 as the solvent and tetramethylsilane as internal standard. Differential scanning calorimetry (DSC) tests were conducted using DSC Q20 (TA Instruments) at a heating rate of 10 °C min−1 under a constant nitrogen flow (50 mL min−1). Dynamic mechanical analysis (DMA) measurements were performed using a TA Instrument DMA Q800 at 1 Hz in three-point bending mode. Specimens, 30 mm × 10 mm × 2 mm (length × width × thickness) were analyzed at a heating rate of 5 °C min−1 under nitrogen. Thermal gravimetric analysis (TGA) was performed with a TGA 4000 (PerkinElmer) system under nitrogen atmosphere from 40 to 500 °C at a heating rate of 10 °C min−1. Tensile testing was conducted using an Instron 5967 with a 30 kN load cell. The dog-bone specimens were tested following ISO standard 8256 type 1BB dimensions. Tests were performed at a crosshead speed of 2 mm min−1. We calculated the tensile modulus over a range of load from 2 N to 18 N.

Results and discussion

All the diol-based thermosets were synthesized as shown Fig. 1, that is, the synthesis of diol-dinorbornenyl-derived monomers and polymerization of the corresponding monomers. All the monomers (i.e., NB2, NB3, NB4, NB5, NB6, NB7, NB8, NB9 and NB10) were synthesized from 5-norbornene-2-carboxylic acid and diols, and the detailed syntheses are given in the ESI. After getting these monomers, this work focused on whether these monomers could be rapidly polymerized completely in the presence of GC2. We first used DSC to study the polymerization behaviour of the diol-derived monomers. After mixing with GC2 (50 ppm per norbornenyl double bond), the resins were probed by DSC, Fig. S1 (ESI).

As can be seen from the DSC curves, all the exothermic peaks were single peaks and appeared below 100 °C. This indicated that these monomers can polymerize at low temperature. The measured exothermic peak temperatures and the amount of heat released (ΔHP) were respectively plotted in Fig. 2(a) and (b). According to Fig. 2(a), a little variation was observed in the exothermic peak temperature, which was located at ∼72 °C. For the amount of heat released, ΔHP increased as the alkyl chain length of the diols increased. For example, the ΔHP s of NB2, NB5 and NB9 were respectively 58.2 kJ mol−1, 70.4 kJ mol−1 and 75.4 kJ mol−1. However, the ΔHP of NB10 decreased compared to that of NB9. Steric structures affect the polymerization, since the driving force of ROMP is the release of strain in the ring structures.36 In this work, steric hindrance was present in the obtained monomers, namely, endo- and exo- diol-derived monomers. This is because there is a combination of isomers (endo- and exo-) in the starting material, 5-norbornene-2 carboxylic acid. To understand the effect of steric hindrance on the polymerization, the ratios of endo- and exo- monomers were calculated by 1H NMR spectroscopy and eqns S-1 and S-2.37 All the monomers exhibited a similar ratio of ∼70/30, implying that steric hindrance had little influence on the polymerization. Diffusion and concentration of the monomers also affect polymerization, therefore, polymerization behaviors of the diol-based monomers varied as the flexible alkyl bridge structures of diols were altered.38–40


image file: d1ma00210d-f2.tif
Fig. 2 (a) Peak temperatures, and (b) heat released from diol-derived monomers in the presence of GC2. Error bars are standard deviation, N = 3.

As mentioned previously, this contribution focused on rapid synthesis of diol-based thermosets, and we synthesized these thermosets at 180 °C for 2 minutes. The issue was whether the diol-derived monomers polymerized completely under the current process? This was investigated by detecting the heat released from the diol-based thermosets using DSC, and the curves are shown in Fig. S2 (ESI). As can be seen, no obvious exothermic peaks were observed, probably suggesting that the diol-derived monomers polymerize completely.

To better explore the polymerization, a control, methyl 5-norbornene-2-carboxylate (NB-Me) was synthesized, and its polymer, PNB-Me, was also synthesized at 180 °C for 2 minutes. DSC (Fig. S3, ESI), FTIR (Fig. 3(a)), 1H NMR (Fig. S4, ESI) and GPC (Fig. S5, ESI) confirmed that NB-Me polymerized completely. In the case of 1H NMR spectrum, for example, cyclic double bond of NB-Me located at 5.92–6.18 ppm41,42 disappeared, and the resonances of acyclic double bonds appeared at 5.33 ppm after polymerization. For FTIR, the bands corresponding to [double bond, length as m-dash]C–H stretching vibration (3142 and 3061 cm−1) and cyclic C[double bond, length as m-dash]C stretching vibration (1625 and 1571 cm−1) of NB-Me disappeared, and new band due to [double bond, length as m-dash]C–H out-of-plane rocking vibration was observed at 970 cm−1 in the spectrum of PNB-Me.43,44 With the aid of this control, polymerization behaviors of the diol-derived monomers were explored by FTIR spectroscopy (Fig. S6, ESI). For these monomers, the peaks located at ∼3128 and ∼3060 cm−1 corresponding to [double bond, length as m-dash]C–H stretching vibration, and ∼1632 and ∼1570 cm−1 assigned to cyclic C = C stretching vibration disappeared after polymerization, while a new absorption by [double bond, length as m-dash]C–H out-of-plane rocking vibration was observed at 970 cm−1. In the case of NB2 (Fig. 3(b)), for instance, absorption at 3128 and 3061 cm−1 disappeared, while new bands appeared at 969 cm−1. This indicated that the diol-based monomers can convert into thermosets quickly under the current process. That is, this work rapidly synthesized diol-based thermosets, and their crosslinked structures are shown in Fig. 1. Interestingly, it is difficult to probe the crosslinked polymers derived from ROMP of norbornene and its derivatives due to their complex architectures, like polydicyclopentadiene. This work may provide a method to explore the structures.


image file: d1ma00210d-f3.tif
Fig. 3 FTIR spectra of (a) NB-Me and PNB-Me, and (b) NB2 and PNB2.

DMA was applied to evaluate the performance of the diol-based thermosets, Fig. S7 (ESI). The data gained from DMA were collected and listed in Table 1. The Tg values of these thermosets exceeded 100 °C. PNB2, PNB3, PNB4 and PNB5 had closer Tg values, and higher than those of PNB6, PNB7, PNB8, PNB9 and PNB10. This is probably caused by the crosslink density which plays an important role in the performance.

Table 1 DMA data of diol-based thermosets
T g (Tan Delta, °C) E′ (298 K, MPa) E′ (Tg+ 40 K, MPa) ρ (× 103, mol m−3)
PNB2 131 1649 147 13.2
PNB3 132 1499 122 11.0
PNB4 129 1255 115 10.4
PNB5 130 1139 127 11.5
PNB6 111 1101 102 9.6
PNB7 103 717 47 4.3
PNB8 106 976 68 6.5
PNB9 112 942 82 7.7
PNB10 102 686 40 3.8


To prove the view, an equation from the statistical theory of rubbery elasticity was applied to estimate the crosslink densities.45,46 This equation can be expressed as

ρ = E′/3RT
where E′ is the storage modulus at 40 K above Tg. T is Tg + 40 K. R is the universal gas constant, 8.314 J (mol K)−1. The crosslink densities of diol-based thermosets were calculated and are shown in Table 1. As can be seen, the crosslink densities were roughly consistent with the variety of the Tg values. Crosslink densities of PNB2, PNB3, PNB4 and PNB5 were higher than those of PNB6, PNB7, PNB8, PNB9 and PNB10. These might be attributed to the alkyl bridge structures of diols.

In order to assess the mechanical properties of these diol-based thermosets, tensile properties were measured, Fig. S8 (ESI). The results are summarized and plotted in Fig. 4. As can be seen, all the thermosets’ tensile strength exceeded 20 MPa, and PNB4 exhibited the best tensile strength (28.2 MPa). For tensile modulus, all these polymers were over 430 MPa, among which PNB3 had the best performance of 655 MPa. In addition, all these polymers showed elongation at break in the range of 7%–12%, implying good toughness. This suggested that the diol-based thermosets have good mechanical properties.


image file: d1ma00210d-f4.tif
Fig. 4 (a) Tensile strength and tensile modulus, and (b) elongation at break of diol-based thermosets. Error bars are standard deviation, N = 5.

Thermal stability of the diol-based thermosets was analyzed by thermogravimetric analysis (TGA). The TGA thermograms are shown in Fig. S9 (ESI), and the data obtained from TGA are listed in Table 2. The 5% and 10% weight loss temperature exceeded 198 and 240 °C, respectively, suggesting that these thermosets have good stability and can be widely applied.

Table 2 Summary of TGA data of diol-based thermosets
T d5 (°C) T d10 (°C)
PNB2 198 240
PNB3 217 240
PNB4 240 333
PNB5 254 385
PNB6 259 389
PNB7 249 380
PNB8 310 394
PNB9 259 385
PNB10 249 366


Table 3 Tensile properties of the composites
PNB5 PNB5C PNB10 PNB10C
Tensile strength (MPa) 27.3 ± 0.9 40.5 ± 2.1 20.1 ± 0.5 35.3 ± 1.8
Tensile module (MPa) 648 ± 26 927 ± 60 469 ± 13 536 ± 43
Elongation at break (%) 7.3 ± 1.2 16.7 ± 1.3 8.2 ± 0.7 24.4 ± 1.8


Due to good mechanical properties, thermal stability and chemical resistance, thermosets are suitable to be used as the matrix of composite components. Diol-derived thermosets can be a potential candidate for the matrix of composites; this work hence also attempted to fabricate the composites. In the case of traditional processing, the manufacture of thermoset components requires the monomer to be polymerized at 180 °C for several hours.47 However, following this work, one can fabricate composites in 2 minutes by polymerizing woven flax fibers infused with the monomer solution because diol-derived monomers can rapidly polymerize. PNB5/woven flax fiber (PNB5C) and PNB10/woven flax fiber (PNB10C) composites were manufactured through vacuum-assisted resin transfer molding (VARTM), Fig. S10 (ESI).

Tensile properties of the composites were also measured, and the representative stress–strain curves are shown in Fig. 5. Tensile strength, tensile modulus and elongation at break of PNB5C were respectively 40.5 MPa, 927 MPa and 16.7%, and those of PNB10C were 35.3 MPa, 536 MPa and 24.4%, respectively. Compared to PNB5 and PNB10 (Table 3), there were great enhancement in the tensile properties. This suggests that diol-based thermosets are good matrices for rapid manufacturing of composites.


image file: d1ma00210d-f5.tif
Fig. 5 Stress–strain curves of the composites.

Conclusions

In summary, this work focuses on rapid manufacturing of diol-based polymers and composites via ROMP. A series of diol-derived monomers were synthesized. These liquid monomers can transform into thermosets at 180 °C in 2 minutes, which benefit the fabrication of composites rapidly through woven flax fibers infused with the monomer solution. Diol homolog-based thermosets exhibited good thermal properties and mechanical properties, and their performance can be enhanced significantly by manufacturing woven flax fiber composites. We believe that diol-based thermosets can be widely used in various fields as a substitute for petroleum-based polymers.

Conflicts of interest

There are no conflicts to declare.

Notes and references

  1. R. Duarah and N. Karak, RSC Adv., 2015, 5, 64456–64465 RSC.
  2. Y. R. Xu, L. F. Guo, H. N. Zhang, H. M. Zhai and H. Ren, RSC Adv., 2020, 10, 22600 RSC.
  3. P. Yang and Y. Gu, J. Polym. Res., 2011, 18, 1725–1733 CrossRef CAS.
  4. R. Hatti-Kaul, L. J. Nilsson, B. Z. Zhang, N. Rehnberg and S. Lundmark, Trends Biotechnol., 2020, 38, 50–67 CrossRef CAS PubMed.
  5. M. A. Hillmyer, Science, 2017, 358, 868–870 CrossRef CAS.
  6. D. K. Schneiderman and M. A. Hillmyer, Macromolecules, 2017, 50, 3733–3750 CrossRef CAS.
  7. Y. Q. Zhu, C. Romain and C. K. Williams, Nature, 2016, 540, 354–362 CrossRef CAS PubMed.
  8. N. Teramoto, Polymers, 2020, 12 DOI:10.3390/polym12102386.
  9. A. Gandini, Macromolecules, 2008, 41, 9491–9504 CrossRef CAS.
  10. A. L. Holmberg, K. H. Reno, R. P. Wool and T. H. Epps, Soft Matter, 2014, 10, 7405–7424 RSC.
  11. R. Mulhaupt, Macromol. Chem. Phys., 2013, 214, 159–174 CrossRef.
  12. K. J. Yao and C. B. Tang, Macromolecules, 2013, 46, 1689–1712 CrossRef CAS.
  13. S. Munoz-Guerra, C. Lavilla, C. Japu and A. M. de Ilarduya, Green Chem., 2014, 16, 1716–1739 RSC.
  14. O. Nsengiyumva and S. A. Miller, Green Chem., 2019, 21, 973–978 RSC.
  15. H. W. Park, M. Toan, H. J. Kim, J. H. Lee and S. Shin, J. Ind. Eng. Chem., 2020, 92, 184–190 CrossRef CAS.
  16. G. Q. Chen and M. K. Patel, Chem. Rev., 2012, 112, 2082–2099 CrossRef CAS PubMed.
  17. H. Yim, R. Haselbeck, W. Niu, C. Pujol-Baxley, A. Burgard, J. Boldt, J. Khandurina, J. D. Trawick, R. E. Osterhout, R. Stephen, J. Estadilla, S. Teisan, H. B. Schreyer, S. Andrae, T. H. Yang, S. Y. Lee, M. J. Burk and S. Van Dien, Nat. Chem. Biol., 2011, 7, 445–452 CrossRef CAS.
  18. J. Lu, L. B. Wu and B. G. Li, ACS Sustainable Chem. Eng., 2017, 5, 6159–6166 CrossRef CAS.
  19. D. Fourcade, B. S. Ritter, P. Walter, R. Schonfeld and R. Mulhaupt, Green Chem., 2013, 15, 910–918 RSC.
  20. K. K. Tremblay-Parrado, C. Bordin, S. Nicholls, B. Heinrich, B. Donnio and L. Averous, Macromolecules, 2020, 53, 5869–5880 CrossRef CAS.
  21. H. Blattmann and R. Mulhaupt, Green Chem., 2016, 18, 2406–2415 RSC.
  22. A. J. Timmis, A. Hodzic, L. Koh, M. Bonner, C. Soutis, A. W. Schafer and L. Dray, Int. J. Life Cycle Assess., 2015, 20, 233–243 CrossRef CAS.
  23. F. Zia, K. M. Zia, W. Aftab, S. Tabasum, Z. I. H. Nazli, M. Mohammadi and M. Zuber, Int. J. Biol. Macromol., 2020, 165, 1889–1899 CrossRef CAS PubMed.
  24. S. Naheed, M. Zuber, M. Barikani and M. Salman, Mater. Sci. Eng., B, 2021, 264 DOI:10.1016/j.mseb.2020.114960.
  25. A. Gallastegui, E. Gabirondo, F. Elizalde, N. Aranburu, D. Mecerreyes and H. Sardon, Eur. Polym. J., 2021, 143 DOI:10.1016/j.eurpolymj.2020.110174.
  26. J. M. Sadler, F. R. Toulan, G. R. Palmese and J. J. La Scala, J. Appl. Polym. Sci., 2015, 132 DOI:10.1002/app.42315.
  27. O. M. Ogba, N. C. Warner, D. J. O’Leary and R. H. Grubbs, Chem. Soc. Rev., 2018, 47, 4510–4544 RSC.
  28. C. W. Bielawski and R. H. Grubbs, Prog. Polym. Sci., 2007, 32, 1–29 CrossRef CAS.
  29. A. E. Madkour, A. H. R. Koch, K. Lienkamp and G. N. Tew, Macromolecules, 2010, 43, 4557–4561 CrossRef CAS PubMed.
  30. J. A. Johnson, Y. Y. Lu, A. O. Burts, Y. Xia, A. C. Durrell, D. A. Tirrell and R. H. Grubbs, Macromolecules, 2010, 43, 10326–10335 CrossRef CAS PubMed.
  31. T. K. H. Trinh, G. Schrodj, S. Rigolet, J. Pinaud, P. Lacroix-Desmazes, L. Pichavant, V. Heroguez and A. Chemtob, RSC Adv., 2019, 9, 27789–27799 RSC.
  32. R. A. Weitekamp, H. A. Atwater and R. H. Grubbs, J. Am. Chem. Soc., 2013, 135, 16817–16820 CrossRef CAS PubMed.
  33. C. W. Cheng, X. H. He, S. M. Huang, F. Zhang, Y. Guo, Y. F. Wen, B. Wu and D. F. Chen, Int. J. Hydrogen Energy, 2020, 45, 19676–19690 CrossRef CAS.
  34. I. M. Rutenberg, O. A. Scherman, R. H. Grubbs, W. R. Jiang, E. Garfunkel and Z. Bao, J. Am. Chem. Soc., 2004, 126, 4062–4063 CrossRef CAS PubMed.
  35. I. D. Robertson, M. Yourdkhani, P. J. Centellas, J. E. Aw, D. G. Ivanoff, E. Goli, E. M. Lloyd, L. M. Dean, N. R. Sottos, P. H. Geubelle, J. S. Moore and S. R. White, Nature, 2018, 557, 223 CrossRef CAS PubMed.
  36. A. H. Hoveyda and A. R. Zhugralin, Nature, 2007, 450, 243–251 CrossRef CAS.
  37. J. M. Pollino, L. P. Stubbs and M. Weck, Macromolecules, 2003, 36, 2230–2234 CrossRef CAS.
  38. Y. Song, S. Zhang and P. Yang, Thermochim. Acta, 2018, 662, 55–63 CrossRef CAS.
  39. Y. Bai, P. Yang, S. Zhang, Y. Q. Li and Y. Gu, J. Therm. Anal. Calorim., 2015, 120, 1755–1764 CrossRef CAS.
  40. E. Skliutas, M. Lebedevaite, E. Kabouraki, T. Baldacchini, J. Ostrauskaite, M. Vamvakaki, M. Farsari, S. Juodkazis and M. Malinauskas, Nanophotonics, 2021, 10, 1211–1242 CrossRef.
  41. C. H. Liu, L. D. Dugas, J. I. Bowman, T. Chidanguro, R. F. Storey and Y. C. Simon, Polym. Chem., 2020, 11, 292–297 RSC.
  42. B. J. Sundell, J. A. Lawrence, D. J. Harrigan, S. B. Lin, T. P. Headrick, J. T. O’Brien, W. F. Penniman and N. Sandler, ACS Macro Lett., 2020, 9, 1363–1368 CrossRef CAS.
  43. T. J. Cuthbert, T. Li, A. W. H. Speed and J. E. Wulff, Macromolecules, 2018, 51, 2038–2047 CrossRef CAS.
  44. H. W. Thompson, D. L. Nicholson and L. N. Short, Discuss. Faraday Soc., 1950, 222–235 RSC.
  45. H. Ishida and D. P. Sanders, J. Polym. Sci. Pol. Phys., 2000, 38, 3289–3301 CrossRef CAS.
  46. L. R. G. Treloar, The physics of rubber elasticity, Clarendon Press, Oxford, 2d ed., 1958 Search PubMed.
  47. D. Abliz, Y. G. Duan, L. Steuernagel, L. Xie, D. C. Li and G. Ziegmann, Polym. Polym. Compos., 2013, 21, 341–348 CAS.

Footnote

Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ma00210d

This journal is © The Royal Society of Chemistry 2021
Click here to see how this site uses Cookies. View our privacy policy here.