Developing new techniques that can synthesize one-dimensional piezoelectric materials on a large scale is of great significance for boosting piezocatalytic applications. In this work, we proposed a high-efficiency template hydrothermal method for large-scale synthesis of piezoelectric Na0.5Bi0.5TiO3 (NBT) nanowires. By ion-exchange with Bi3+, Na2Ti3O7 template nanowires can be easily and entirely transformed to NBT. The piezocatalytic activity of the NBT nanowires was thoroughly investigated with respect to their capability to degrade typical organic pollutants, including Rhodamine B, methylene blue, methyl orange, tetracycline hydrochloride, phenol, and bisphenol A. The NBT nanowires exhibited the highest efficiency in piezocatalytic degradation of Rhodamine B, which was completely decomposed within 80 min (rate constant ∼0.0575 min−1). The electron spin resonance spin-trapping technique and active species capture experiments were employed to characterize free radicals. The present work is advantageous for the high yield of NBT nanowires and the excellent piezocatalytic performance. The reported template hydrothermal method can potentially be extended to the synthesis of other perovskite nanowires.
Representative piezocatalysts include BaTiO3,10 Pb(Zr0.52Ti0.48)O3,11 Pb(Mg1/3Nb2/3)O3–xPbTiO3,12 Bi2WO6,13 KNbO3,14 and NaNbO3,15 which have been proved to be effective in degrading various organic pollutants. Unfortunately, most of the reported piezocatalysts suffer from low efficiency in actual applications. Much effort has been devoted to improving the functional performance of piezocatalysts. It is generally believed that the large piezo-electric coefficient, highly flexible structure and abundant active sites of piezocatalysts are beneficial. More recently, electrical conductivity was regarded as another vital factor that influenced the piezocatalytic performance.16–19 It was suggested that the high electrical conductivity helped to accelerate charge transfer in the piezocatalytic process and thus enhanced the piezocatalytic activity.20
Na0.5Bi0.5TiO3 (NBT) is an attractive piezoelectric material because of its large piezoelectric coefficient (d33 value of ∼58 pC N−1)21,22 and high Curie temperature (340 °C).23 In addition, it is reported that the relatively high electrical conductivity (∼10−5 S m−1) of NBT may be favorable for piezocatalytic applications.20 Recently, research studies on the piezocatalytic performance of NBT have been carried out.24–26 It is worth noting that most of the reported NBT piezocatalysts are microparticles24 or multi-crystalline nanofibers.25 The piezocatalytic performance of NBT single-crystalline nanowires has never been reported. It is highly expected that single-crystalline nanowires may have higher piezocatalytic activity because of their higher flexibility and larger specific surface area.
In this work, NBT single-crystalline nanowires with uniform morphology were prepared via a template hydrothermal method using Na2Ti3O7 nanowires as the template. The piezocatalytic activity of the NBT nanowires was evaluated from the degradation efficiency for different kinds of organic pollutants. Piezocatalytic mechanisms were also systematically investigated through quenching experiments and ESR characterization. This study may open up a promising approach to design and synthesize piezoelectric nanowires for environmental purification.
The NBT nanowires were subsequently synthesized through a hydrothermal reaction, in which the prepared Na2Ti3O7 nanowires were employed as a Ti4+ source and Bi(NO3)3·5H2O was employed as a Bi3+ source. First, 0.4851 g of Bi(NO3)3·5H2O and 0.2010 g of Na2Ti3O7 were dispersed in NaOH solution. The mixed solution was then sonicated for 20 min and stirred for 30 min to form a uniform suspension. The final mixture was hydrothermally treated at 200–240 °C for 6–24 h in a 100 mL Teflon-lined stainless-steel autoclave with a 70% filling factor. The reaction temperature, reaction time, and mineralizer concentration for the synthesis of pure NBT nanowires were investigated in detail. After the reaction, the formed white precipitate was collected by centrifugation, washed several times with distilled water and 0.2 mol L−1 acetic acid, and finally dried at 60 °C for 12 h.
Furthermore, the electron spin resonance (ESR) technique was also employed to detect active free radicals such as radical ·OH and radical ·O2− with the assistance of 5,5-dimethyl-1-pyrroline N-oxide (DMPO). ESR investigations were conducted on a Bruker A300-10-12 spectrometer. Specifically, for the detection of radical ·OH, the as-prepared sample was dispersed in deionized water, and for the detection of radical ·O2−, the as-prepared sample was dispersed in dimethyl sulphoxide (DMSO).
Fig. 1 schematically depicts the processing steps for growing NBT nanowires. In the first step, Na2Ti3O7 nanowires were prepared via a simple hydrothermal method. In the following step, Na2Ti3O7 and Bi(NO3)3·5H2O were added to NaOH solution. During the reaction, Bi3+ ions will reduce the stability of the layered titanate Na2Ti3O7 and break the connection between the TiO6 octahedra.34 The dissociated TiO6 octahedra will then react with Bi3+ and Na+ ions to form perovskite-type NBT.
The XRD pattern of the synthesized Na2Ti3O7 nanowires is shown in Fig. S1,† which demonstrates that pure-phase Na2Ti3O7 (JCPDS No. 31–1329) has been formed. Fig. 2a–c show the XRD patterns of the NBT samples prepared under different reaction conditions. As shown in Fig. 2a, a composed phase structure was obtained in the samples synthesized at lower NaOH concentrations (3–5 mol L−1). The major phase can be identified as NBT with a monoclinic or pseudo hexagonal structure (JCPDS No. 46-0001), and the additional peaks can be ascribed to Na5Bi4.5Ti4O15. When increasing the NaOH concentration to 10 mol L−1, the secondary phase disappeared completely, and pure-phase NBT was obtained. Fig. 2b illustrates the influence of reaction temperature (200–240 °C) on the phase constitution of the product. The NaOH concentration was 10 mol L−1. In the synthesis at 200 °C for 24 h, the NBT phase was formed along with Na2Ti3O7 and Bi2O3 secondary phases. The pure-phase product was obtained by increasing the reaction temperature to over 220 °C. Based on these results, one may conclude that the high mineralizer concentration and high reaction temperature are beneficial for the hydrothermal synthesis of NBT. We found that the reaction time (6 h to 24 h) has little influence on the phase constitution of the hydrothermal product (Fig. 2c). For the NBT samples synthesized after 12 hours (NBT-12), the peak intensity of (110) and (220) was slightly enhanced, which may be due to the fact that the NBT-12 samples were a mixture of nanobelts and nanoparticles (Fig. S2†). The larger area of nanobelts results in the (100) and (200) facets being more easily scanned by X-ray. The NBT samples obtained from the 24 h-synthesis are crystallized into micro-scale particles (Fig. S3†). Pure-phase NBT nanowires were finally obtained by reducing the hydrothermal reaction time to 6 h.
The morphology of the pure-phase NBT nanowires can be clearly observed by SEM. Fig. 3a shows the SEM image of the Na2Ti3O7 template nanowires, which are straight and smooth with an average lateral dimension of ∼250 nm and a longitude larger than 5 μm. After reacting with Bi(NO3)3 solution, the Na2Ti3O7 template nanowires were entirely transformed to uniform and slender NBT nanowires (Fig. 3b). The lateral dimension of the nanowires is about 100 nm. The distribution of elements in the NBT nanowires was analyzed by the EDX spectroscopy elemental mapping technique. As shown in Fig. 3c, all the involved elements (Bi, Na, Ti, and O) are homogeneously distributed and well-matched with each other. The analytical composition of the obtained Na0.5Bi0.5TiO3 was characterized using EDS spectra (Fig. S4†), in which the ratio of Na, Bi, and Ti in NBT nanowires is 22.2:22.8:55. The TEM images (Fig. 3d–e) illustrate the straight and smooth surface of the NBT nanowires, indicating the high-quality of the present material. The amplified HRTEM image (Fig. 3f) taken from the selected area of Fig. 3e shows clear lattice fringes of (113) planes (d = 1.78 Å), which are oriented along the extension direction of the nanowire.
Fig. 3 SEM images of (a) Na2Ti3O7 and (b) Na0.5Bi0.5TiO3 nanowires; (c) EDS mapping, (d and e) TEM, and (f) HRTEM of Na0.5Bi0.5TiO3 nanowires. |
XPS investigation was carried out to elucidate the valence state of the as-prepared NBT nanowires. The full survey XPS spectrum in Fig. S5† clearly shows the existence of Na, Bi, Ti and O elements in the sample. The high-resolution XPS spectrum of Na 1s (Fig. 4a) shows a peak at 1070.75 eV. Fig. 4b presents two main peaks at 158.75 and 164.05 eV, which correspond to Bi 4f7/2 and Bi 4f5/2, respectively. Fig. 4c shows the high-resolution XPS spectrum of Ti 2p. The Ti 2p3/2 and Ti 2p1/2 peaks are located at 457.9 eV and 464 eV, respectively, in accordance with the data of Ti4+. The XPS spectrum of O 1s in Fig. 4d is deconvoluted into three peaks, which can be assigned to lattice oxygen (OL, 529.2 eV), defective oxygen (OV, 531.1 eV) and surface adsorbed oxygen (OC, 533.8 eV), respectively.35 The presence of oxygen vacancies could efficiently promote the adsorption and activation of O2 on the surface of the piezocatalyst and consequently enhance piezocatalytic activity.36 Therefore, it is speculated that the oxygen vacancy defects in NBT may contribute to its excellent piezocatalytic performance. However, the effect of oxygen defects on the energy band structure and the mechanism of improving the piezocatalytic performance need to be further studied.
Fig. 4 High-resolution XPS spectra of the as-prepared Na0.5Bi0.5TiO3 nanowires: (a) Na 1s, (b) Bi 4f, (c) Ti 2p, and (d) O 1s. |
PFM testing was employed to characterize the piezoelectricity of the prepared NBT nanowires. The experimental setup of PFM is illustrated in the inset of Fig. 5a. By applying a tip bias of ±3 V, localized point-to-point piezo-responses of the samples were probed. The PFM amplitude–voltage butterfly curve and phase–voltage hysteresis loop are given in Fig. 5. The butterfly-shaped curve appears symmetrical, indicating the certain piezoelectric properties. On the other hand, the phase hysteresis loop presents about 180° domain switching at ±3 V (Fig. 5b).
Fig. 5 (a) Amplitude butterfly curve (the inset: experimental setup of PFM) and (b) phase hysteresis of NBT NWs. |
To study the piezocatalytic performance of NBT nanowires, diverse industrial pollutants, including anionic dyes (RhB and MB), a cationic dye (MO), and neutral stubborn pollutants (TH, BPA and phenol), are used as target contaminants. Fig. 6a–f display the typical absorption spectra of the aqueous solutions of these pollutants. Piezocatalytic experiments without using NBT were carried out. It was clear that the pollutants could hardly be degraded without NBT under ultrasonic vibration. After being treated with ultrasonic vibration for 80 min, RhB, MO, MB, TH, BPA and phenol were removed 100%, 92.8%, 66.7%, 65.7%, 60.6% and 58.5% (Fig. 6g), respectively. The results demonstrated that the NBT nanowires are effective in degrading various kinds of organic pollutants. The first-order rate constants for the piezocatalytic degradation of the target pollutants were evaluated by refinement of the ln(C0/C) − t plot (Fig. 6h). The results are presented in Fig. 6i. The highest rate constant (0.0575 min−1) was obtained for RhB. The piezocatalytic performance of NBT samples in this work was compared with that of other reported NBT materials. As shown in Table 1, the NBT nanowires prepared by the template hydrothermal method show the highest piezocatalytic performance.
To distinguish the role of active radicals in the piezocatalytic degradation of MO over NBT, trapping experiments were conducted using TBA, BQ and EDTA–2Na as radical scavengers. As revealed in Fig. 7a and b, the piezocatalytic performance was inhibited greatly upon introducing TBA, which indicated that ·OH was the primary active species. Furthermore, the piezocatalytic oxidation ability of NBT was also restrained by the addition of BQ and EDTA, indicating that ·O2− and h+ played an auxiliary role in the piezocatalytic degradation of MO over NBT. ESR characterization was carried out to confirm the existence of ·OH and ·O2−. The nitrone spin trap 5,5-dimethyl-1-pyrroline N-oxide (DMPO) was introduced into the aqueous and dimethyl sulphoxide (DMSO) dispersions of the NBT catalyst for probing hydroxyl radicals (·OH) and superoxide radicals (·O2−), respectively. Well-defined signals (Fig. 7c and d) of the specific DMPO–·OH and DMPO–·O2− adducts were observed after being treated with ultrasound for 5 minutes. These results confirmed the generation of ·OH and ·O2− radicals in the piezocatalytic process.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1na00024a |
This journal is © The Royal Society of Chemistry 2021 |