aInstitute for Materials Science, Max Bergmann Centre of Biomaterials, Dresden Center for Nanoanalysis, TU Dresden, 01062, Dresden, Germany. E-mail: nadia.licciardello@tu-dresden.de; nadia.licciardello@inl.int; gianaurelio.cuniberti@tu-dresden.de
bIT4Innovations, VŠB – Technical University of Ostrava, 17. listopadu 15/2172, 708 33 Ostrava, Czech Republic
cNanotechnology Centre, CEET, VSB-Technical University of Ostrava, 17. listopadu 15/2172, 708 33 Ostrava, Czech Republic
dInstitute of Inorganic Chemistry, Czech Academy of Sciences, Husinec-Řež 1001, 250 68 Řež, Czech Republic
First published on 13th April 2021
Antibiotics in wastewater represent a growing and worrying menace for environmental and human health fostering the spread of antimicrobial resistance. Titanium dioxide (TiO2) is a well-studied and well-performing photocatalyst for wastewater treatment. However, it presents drawbacks linked with the high energy needed for its activation and the fast electron–hole pair recombination. In this work, TiO2 nanoparticles were decorated with Ag nanoparticles by a facile photochemical reduction method to obtain an increased photocatalytic response under visible light. Although similar materials have been reported, we advanced this field by performing a study of the photocatalytic mechanism for Ag–TiO2 nanoparticles (Ag–TiO2 NPs) under visible light taking in consideration also the rutile phase of the TiO2 nanoparticles. Moreover, we examined the Ag–TiO2 NPs photocatalytic performance against two antibiotics from the same family. The obtained Ag–TiO2 NPs were fully characterised. The results showed that Ag NPs (average size: 23.9 ± 18.3 nm) were homogeneously dispersed on the TiO2 surface and the photo-response of the Ag–TiO2 NPs was greatly enhanced in the visible light region when compared to TiO2 P25. Hence, the obtained Ag–TiO2 NPs showed excellent photocatalytic degradation efficiency towards the two fluoroquinolone-based antibiotics ciprofloxacin (92%) and norfloxacin (94%) after 240 min of visible light irradiation, demonstrating a possible application of these particles in wastewater treatment. In addition, it was also proved that, after five Ag–TiO2 NPs re-utilisations in consecutive ciprofloxacin photodegradation reactions, only a photocatalytic efficiency drop of 8% was observed. Scavengers experiments demonstrated that the photocatalytic mechanism of ciprofloxacin degradation in the presence of Ag–TiO2 NPs is mainly driven by holes and ˙OH radicals, and that the rutile phase in the system plays a crucial role. Finally, Ag–TiO2 NPs showed also antibacterial activity towards Escherichia coli (E. coli) opening the avenue for a possible use of this material in hospital wastewater treatment.
Among semiconductor materials, TiO2 is one of the most used photocatalysts because of its large specific surface area, relatively low toxicity, low cost and high catalytic activity.24 In 1972, Fujishima and Honda were the first to report the photocatalytic activity of TiO2, which was used as the photo-anode in UV-light induced electrochemical water splitting.25 Ever since, this material has been widely explored in photocatalysis for several applications, including wastewater treatment. However, TiO2, especially in its more commonly used crystalline phase anatase, has a wide bandgap (∼3.2 eV), which requires UV light irradiation for the photo-activation. UV light contribution in solar irradiance spectrum is limited (5%) compared to visible (43%) and infrared light (52%), which restricts TiO2 actual environmental application under visible or solar light irradiation.26
Doping TiO2 with metal or non-metal atoms or modifying the surface of TiO2 with noble metals are some of the suggested solutions to overcome this problem.27–31 Noble metals play an important role in the visible-light-activated photocatalytic process24,32 by lowering the bandgap, promoting electron–hole pairs separation and/or introducing additional catalytically active sites on the surface of TiO2. Among them, Ag is a promising candidate, owing to its relatively low cost (compared with gold for instance), easy preparation and particularly high performance in enhancing the TiO2 photocatalytic activity under visible light.33 When the TiO2 surface is decorated with Ag NPs, the photocatalytic response under visible light is enhanced because of the localised surface plasmon resonance effect of Ag NPs and the increased separation efficiency of photogenerated electron–hole pair, since Ag can act as an electron acceptor.4,34 Besides, Ag NPs have a long-time known strong antibacterial activity.4
However, a deep understanding of the photocatalytic mechanism for Ag–TiO2 NPs under visible light irradiation is often missing in the literature35,36 and authors usually ignored the role played by the rutile phase of TiO2 when using commercial TiO2 P25.37
In this manuscript, we report on the surface modification of the commercial Evonik Aeroxide® TiO2 P25 with Ag nanoparticles using a facile photochemical reduction method.38 The phase composition and microstructure as well as the optical properties of the as-obtained Ag–TiO2 NPs were analysed. The photocatalytic performance under visible light irradiation for the photodegradation of the fluoroquinolone-based antibiotics CIP and NFX was explored. The possibility to reuse the same batch of Ag–TiO2 NPs was examined. As a model, the photocatalytic mechanism underlying the degradation of CIP in the presence of Ag–TiO2 NPs was investigated shedding some light on it, and taking into consideration the role played by the rutile phase. Moreover, qualitative experiments on the antibacterial activity of the Ag–TiO2 NPs against E. coli were also performed, showing antimicrobial ability and demonstrating the potential disinfection properties of these particles in addition to their photocatalytic activity. These findings not only contribute to better explain the mechanism behind the photocatalytic activity of Ag–TiO2 NPs under visible light, but envisage the prospective future use of these particles, for instance, in hospital wastewater treatment, where both bacteria and pharmaceuticals might be present.
The chemical composition of Ag–TiO2 NPs was examined via Attenuated Total Reflectance-Fourier Transform Infrared (ATR-FTIR) spectroscopy. ATR-FTIR spectra were recorded on IRAffinity-1S (Shimadzu, Japan) equipped with GladiATR-10 as ATR accessory. The spectra were acquired in transmission mode, acquiring 32 scans with a resolution of 2 cm−1 in the wavenumber range from 4000 to 500 cm−1.
The crystalline structure of the prepared Ag–TiO2 NPs was investigated by X-ray powder diffraction (XRD). XRD patterns were obtained by Bruker D8 Advance diffractometer with λCu = 0.15406 nm. Prepared powder samples were placed into a rotational holder.
The measurement of optical absorption and bandgap energies was obtained by diffuse reflectance UV-Vis (UV-Vis DRS) spectra in the range of 280–800 nm with a Shimadzu spectrophotometer UV-2600. The obtained spectra were measured in diffuse reflectance mode and expressed in terms of absorbance by means of Kubelka–Munk function.
The Fluorometer FLS920 (Edinburgh Instrument Ltd, UK), equipped with a 450 W xenon lamp, was used for the acquisition of photoluminescence spectra. The excitation wavelength 325 nm was used for all the measurements. All the samples were measured in powdered form.
Specific surface area (ABET) was measured with the surface area analyser SA9601 (HORIBA Scientific, Japan). The dry powdered samples were degassed for 6 hours at 80 °C, and subsequently the six-point analysis was applied.
The photocatalytic activity of TiO2 P25 and Ag–TiO2 NPs catalysts was evaluated by the chemical degradation of CIP and NFX antibiotics. In detail, 15 mg of catalyst were added to 50 mL of antibiotic solution (CIP or NFX) to reach a catalyst concentration of 300 mg L−1. The antibiotic solution had an initial concentration of 3 mg L−1 (pH = 3, adjusted by using 1 M HCl). The selection of pH = 3 for the CIP and NFX solutions was performed to ensure better solubility of the antibiotics in water. According to the literature, indeed, the CIP and NFX have two acid dissociation constant (pKa) values of 5.9 and 8.9 for CIP, and 6.4 and 8.7 for NFX. Therefore, they are positively charged at pH = 3,39 which increases their solubility in water.
As visible light source, an artificial lamp was used (Ingenieurbüro Mencke & Tegtmeyer GmbH, Germany) with Susicontrol software (version 2.9.0) to monitor the light intensity by a silicon irradiance sensor. As reported by the producer, the visible light spectrum is similar to the natural solar light, but with negligible UV light content (wavelengths ranging from 400 to 1100 nm). The irradiance used during the experiments was 98 W m−2. The distance between the visible light source and the surface of the CIP or NFX solution was 9.4 cm. The catalyst particles were added into the CIP or NFX solution under stirring. The mixture was kept in dark conditions for 30 min to establish the adsorption–desorption equilibrium before irradiation with visible light. The absorbance changes for CIP and NFX were monitored at 277 nm (for CIP) or 278 nm (for NFX) at different times of irradiation by using a UV-Vis spectrophotometer. During the process, samples were withdrawn at times 0 min (before irradiation) and after 5 min, 10 min, 20 min, 30 min, 50 min, 70 min, 90 min, 120 min, 150 min, 180 min, 210 min, 240 min of visible light irradiation and centrifuged for 20 min at 20817g and 20 °C, in order to remove the suspended nanoparticles.
A similar procedure was followed for the recycling experiments: after each CIP photocatalytic degradation, the Ag–TiO2 NPs were recovered by centrifugation (10 min at 20817g), washed once with 0.1 M HCl and twice with ultrapure water, dried at 40 °C in the oven and reused for the subsequent photocatalytic degradation of fresh CIP solution.
Besides, in order to study the photocatalytic degradation mechanism of CIP by Ag–TiO2 NPs, different scavengers, namely EDTA (17 mg), isopropanol (5 mL) and AgNO3 (17 mg), were introduced into the system (total volume 50 mL) as holes (h+) scavenger, ˙OH radicals scavenger, and electrons (e−) scavenger, respectively.
The E. coli suspension culture was prepared as follows. Firstly, 10 g of LB broth was added to 500 mL of ultrapure water in a sterile flask under stirring for 15 min. Secondly, the LB broth was sterilised in the autoclave and subsequently cooled to room temperature. Subsequently, 50 mL of LB broth were transferred to a new sterile flask to which 2 mL of the E. coli culture were added while working in the laminar flow chamber. Finally, this solution was incubated overnight under continuous shaking at 37 °C.
In order to prepare the LB agar plate, 10 g of LB broth, 7.5 g of Agar–agar were added to 500 mL of ultrapure water in a sterile flask under stirring for 15 min. The medium was afterwards sterilised in the autoclave and subsequently cooled down. Finally, a sufficient volume of the LB-agar was transferred into a sterile Petri dish while working in the laminar flow chamber. The as-prepared LB agar plate was stored at 4 °C for future use.
The antibacterial activity of Ag–TiO2 NPs against E. coli was evaluated by a modified streaking method.40,41 The specific experimental steps are as follows. The LB agar plate was divided into two parts by using an antibacterial stick. Five streaks were made for each part. A solution of E. coli in LB broth (20 μL, 108 cells per mL) was placed in each streak on the left part of the plate. Ag–TiO2 NPs (0.2 mg) and E. coli in LB broth (20 μL, 108 cells per mL) were placed in each streak on the right part of the plate. The obtained plate was incubated in dark conditions at 37 °C for 24 h, and examined for testing the strain inhibition in the presence of Ag–TiO2 NPs. As a comparison, another LB agar plate was divided into two parts by using the antibacterial stick. Five streaks were made for each part. E. coli bacteria in LB broth (20 μL, 108 cells per mL) were placed in each streak on the left part of the plate. TiO2 P25 (0.2 mg) and E. coli in LB broth (20 μL, 108 cells per mL) were placed in each streak on the right part of the plate. The obtained plate was incubated in dark conditions at 37 °C for 24 h, and examined for testing the strain inhibition in the presence of TiO2 P25.
The ATR-FTIR spectra of TiO2 P25 and Ag–TiO2 NPs are shown in Fig. S1 (ESI†) and confirm that the Ag NPs did not modify the chemical structure of TiO2 P25. However, the concentration of Ag NPs compared with TiO2 NPs in the sample is very low and it is therefore difficult to confirm their presence by FTIR spectroscopy. In order to prove the presence of Ag NPs in the Ag–TiO2 NPs system, the sample was thus characterised by XRD. The XRD patterns of TiO2 P25 and Ag–TiO2 NPs are shown in Fig. 1.
Fig. 1 Powder XRD patterns of TiO2 P25 and Ag–TiO2 NPs. The blue lines represent the diffraction peaks positions for the typical Ag XRD pattern (JCPDS no. 87-0717). |
The XRD pattern for the TiO2 P25 shows several typical peaks for both anatase and rutile, as expected. Besides the diffraction pattern similar to the one of TiO2 P25, the Ag–TiO2 NPs exhibit four additional main diffraction peaks at 38.116°, 44.277°, 64.426° and 77.472°. These peaks correspond to the (111), (200), (220) and (311) planes of Ag (JCPDS no. 87-0717; the blue bars in Fig. 1).42 These results prove that the obtained Ag–TiO2 NPs contain Ag. Furthermore, the estimated weight percentages of anatase, rutile and silver based on the XRD patterns are 82.12%, 12.76% and 5.12% respectively. The morphology and structure of Ag–TiO2 NPs were characterised by HRTEM measurements. Fig. 2(a) shows the HRTEM image of Ag–TiO2 NPs, where the Ag NPs are observed as darker and smaller dots on the TiO2 NPs surface. As it is shown in Fig. 2(a), the Ag NPs are very finely and homogeneously dispersed on the TiO2 surface.
Fig. 2 (a) HRTEM image of Ag–TiO2 NPs; (b) EDS map of Ag–TiO2 NPs with Ag (red) and Ti (green) atomic distribution; (c) EDS map of Ag–TiO2 NPs with Ag atomic distribution (in red). |
The size distribution of Ag NPs is shown in Fig. S2.† The average size of the Ag NPs is 23.9 ± 18.3 nm. However, these represent probably the agglomerated primary Ag NPs present in higher amount and more easily individuated by HRTEM. From the size distribution graph in Fig. S2(b),† it is clear that the primary Ag NPs size lies between 10 and 20 nm, although also smaller particles are visible in the STEM-HAADF micrograph in Fig. S2(a).† Some Ag NPs agglomerates with size bigger than 100 nm are also present. The EDS elemental maps are shown in Fig. 2(b) and (c). From these maps, it is even more evident that Ag NPs are localised mainly at the surface of the TiO2 NPs. The successfully Ag modification on the surface of TiO2 was confirmed by EDS analysis, where the weight percentage of Ag is about 5%, which is a similar result to the one obtained by XRD patterns.
Fig. 3(a) and (b) clearly show that Ag NPs are evenly distributed on the surface of TiO2. The SAED image in Fig. 3(c) shows the crystalline lattice of TiO2 NPs displaying the lattice spacing of 0.351 nm, 0.175 nm and 0.118 nm, which are characteristics for the crystalline planes (011), (022) and (008), respectively. Besides, in the SAED image, it is also possible to individuate the lattice spacing of 0.235 nm for the (111) planes of Ag NPs.
Fig. 3 HRTEM images at low magnification (a) and high magnification (b) of Ag–TiO2 NPs; (c) SAED (selected area electron diffraction) pattern of Ag–TiO2 NPs. |
UV-Vis diffuse reflectance spectroscopy was used to investigate optical absorption and bandgap energy of both TiO2 P25 and Ag–TiO2 NPs. Fig. 4(a) shows the DRS spectra of pure TiO2 P25 and Ag–TiO2. Both materials show the typical absorption edge in the UV region around 380 nm. However, in the case of Ag–TiO2 NPs, the spectrum contains a broad band in the visible region ranging from 385 to 800 nm with the maximum absorbance in the range between 530 and 550 nm, that is ascribable to the localised surface plasmon resonance (LSPR) of Ag particles.43 The position of the maximum absorbance around 540 nm could be influenced by the used Ag precursor in the Ag–TiO2 NPs synthesis. Albiter et al.44 studied the synthesis of Ag–TiO2 NPs in the presence of different Ag precursors, and they found out that the maximum absorbance in the visible light region strongly depended on the chosen salt for synthesis. Moreover, the position of the maximum absorbance is influenced by particle size, particles distribution on the surface of TiO2 and chemical interaction between Ag NPs and TiO2.44 The DRS spectra also represent an indirect proof of the TiO2 surface coverage with Ag NPs, since the obtained spectra resemble the plasmon surface absorption typical of Ag NPs.45 Similar effects, caused by TiO2 NPs' surface decoration with Ag NPs, on the absorption properties of the final system were already observed in other reported Ag–TiO2 NPs samples.35
Fig. 4 (a) UV-Vis absorption spectra of TiO2 P25 and Ag–TiO2 NPs with the inset of Tauc plot and (b) PL spectra of TiO2 P25 and Ag–TiO2 NPs. |
Furthermore, Ag NPs at the interface with TiO2 slightly shifted the electronic bandgap of TiO2 to higher wavelength due to the creation of a metal–semiconductor junction (Schottky contact). The estimated bandgap energy for TiO2 P25 is 3.28 eV, corresponding to an absorption edge around 378 nm, while in the case of Ag–TiO2 NPs, the estimated bandgap energy is around 3.2 eV (387.5 nm). Thus, the surface decoration of TiO2 with Ag NPs slightly affected the bandgap energy of TiO2. However, it is evident that the photo-response of the Ag–TiO2 NPs is greatly enhanced in the visible light region when compared to bare TiO2.
To investigate the promoted electron–hole pairs separation and the recombination of these photo-excited carriers, the emission spectra of the samples were acquired (λexc = 325 nm, Fig. 4(b)). A lower emission intensity is desirable as it might indicate a lower probability of electron–hole recombination and an enhanced longer lifetime of the photogenerated charge carriers resulting in higher photocatalytic activity. As shown in Fig. 4(b), both TiO2 P25 and Ag–TiO2 NPs show the maximum photoluminescence (PL) emission intensity around 428 nm, but the intensity is lowered by 40% for Ag–TiO2 NPs demonstrating a lower electron–hole recombination rate in this material in respect to TiO2 P25. Similar PL results are reported for Ag/TiO2 (ref. 46) and Ag2O/TiO2 (ref. 47) systems.
Finally, the specific surface area (SSA) of TiO2 P25 and Ag–TiO2 NPs were measured to be 67 and 66 m2 g−1, respectively, showing that the surface area of pure TiO2 nanoparticles was practically unchanged by the introduction of Ag NPs. This indirectly proofs that the photocatalytic activity of Ag–TiO2 NPs under visible light will not be different from the one of pure TiO2 P25 NPs because of a change in surface area, as shown in the next section.
The photocatalytic performance of Ag–TiO2 NPs was initially evaluated by measuring the degradation of CIP in aqueous solution. Moreover, commercial TiO2 P25 was used as a reference. Before the photocatalytic experiment, photocatalysts were kept in contact with the antibiotic in dark conditions for 30 min to reach the adsorption–desorption equilibrium. The results showed, as expected, that there was no significant change in the pollutant concentration in dark conditions, which indicated that an adsorption–desorption equilibrium was reached after 30 minutes. Also, the concentration of CIP did not significantly change under visible light irradiation in the absence of the photocatalyst (Fig. S4(a) in ESI†), demonstrating the negligible photolysis of this molecule under visible light and the crucial role of the photocatalyst in the degradation of CIP in these conditions (Fig. 5(b)). Significant degradation of CIP, as it will be described more in detail below, occurs in the presence of both photocatalysts (TiO2 P25 and Ag–TiO2 NPs) under visible-light irradiation (Fig. 5(b)), as similarly reported in the literature.48 Nevertheless, from Fig. 5(b) it is already evident that the degradation of CIP is much faster in the presence of Ag–TiO2 NPs when compared to the TiO2 P25 reference. Fig. 5(a) shows that the UV-Vis maximum absorbance of CIP decreases with the increase of the irradiation time with visible light in the presence of Ag–TiO2 NPs. In particular, the concentration of CIP is decreased by 92% in the presence of Ag–TiO2 NPs after 240 min irradiation. Differently, within the same time, TiO2 P25 degraded only 67% of CIP, a value comparable to previously reported results.15,49 The high visible light photocatalytic activity of Ag–TiO2 NPs can be attributed to the optical properties of the system induced by the presence of the finely distributed Ag NPs on the surface of TiO2.
In order to investigate the photocatalytic activity of Ag–TiO2 NPs thoroughly, a kinetic study of the photodegradation process was performed. The obtained photocatalytic degradation curve was fitted by using a pseudo-first-order kinetic model as in eqn (1):32
(1) |
Catalyst | kCIP (10−3 min−1) | kNFX (10−3 min−1) |
---|---|---|
TiO2 P25 | 3.7 | 4.6 |
Ag–TiO2 NPs | 7.6 | 7.9 |
We selected NFX as a second target compound to evaluate the visible light photocatalytic activity of Ag–TiO2 NPs. The concentration of NFX did also not significantly change under visible light irradiation in the absence of the photocatalyst (Fig. S4(b) in ESI†). As for CIP, the photodegradation of NFX using Ag–TiO2 NPs was studied by acquiring the absorption spectra of the NFX solution at different times of visible light irradiation in the presence of the photocatalyst, as shown in Fig. 6(a). In Fig. 6(b), the variation of NFX concentration over time shows that after 240 min of visible light exposure, the concentration of NFX decreased by 94% in the presence of Ag–TiO2 NPs and 76% in the presence of TiO2 P25. The pseudo-first-order-kinetic fitting (Fig. S5(b)† and Table 1) indicates that the degradation rate constant for Ag–TiO2 NPs is about 1.7 times higher than that for TiO2 P25. The degradation rate constants reported for similar catalysts, which were used in the photodegradation of CIP under similar irradiation conditions, are in the same range or even have lower values when compared with our findings.32,50 Higher degradation rate constants were also reported, but in this case the materials were either exhibiting different morphologies and/or Ag loading, or were tested under different irradiation conditions.15,51,52 Concerning NFX, a direct comparison of our catalysts performance with respect to the literature is rather difficult since the reported catalysts for the degradation of NFX possess different morphologies or are used in different experimental conditions.53,54 Based on our results, it can be concluded that the decoration of TiO2 surface with Ag NPs can significantly enhance the photocatalytic activity, under visible light irradiation, of the TiO2 P25 towards CIP and NFX.
Finally, we performed the recycling photocatalytic experiments to assess the photocatalytic performance of Ag–TiO2 NPs over different photocatalytic cycles. We chose CIP as a model pollutant for this experiment since it is the most commonly used antibiotic of its family and since we further studied the photocatalytic mechanism for this pharmaceutical in this work.
The results for five photocatalytic cycles are reported in Fig. 7. Ag–TiO2 NPs were utilised in the photocatalytic degradation of CIP, recovered, washed once with 0.1 M HCl, twice with ultrapure water, and dried before being used for another photocatalytic experiment with a fresh CIP solution. This procedure was repeated five times.
Fig. 7 Five photocatalytic degradation reactions of fresh CIP solution (3 mg L−1, pH = 3) with reused (for up to 5 cycles) Ag–TiO2 NPs (300 mg L−1) under visible light irradiation. |
As shown in Fig. 7, the visible-light photocatalytic efficiency of Ag–TiO2 NPs towards CIP only slightly decreased with the number of reutilisations. After five cycles, the amount of degraded CIP decreased only by 8%, namely from 91% to 83% of the initial CIP amount. The small decrease in the photocatalytic efficiency may be due to the loss of active sites caused by the adsorption on the surface of the catalyst of possibly unreacted CIP and/or its degradation products. The results obtained in this work are good and fit well with the previously published findings for similar catalysts, where comparable or even larger drops in catalyst efficiency were observed after cycling.55–57 Our results indicate that the prepared Ag–TiO2 NPs possess high stability and durability thus opening the path, after further studies, for a possible future industrial application.
Fig. 8 shows that the photocatalytic degradation percentage of CIP by Ag–TiO2 NPs in the absence and the presence of different scavengers. When EDTA, a scavenger for holes (h+), was added into the reaction system, CIP degradation was significantly inhibited, and no CIP was degraded after 240 min irradiation. Another evident inhibition phenomenon for the photocatalytic reaction occurred in the presence of isopropanol, a scavenger for ˙OH radicals. Indeed, when isopropanol was added into the reaction system, the degradation efficiency of Ag–TiO2 NPs towards CIP decreased, resulting in 55% CIP degradation after 240 min irradiation. In contrast, in the case of the addition of AgNO3, a scavenger for electrons (e−), the photocatalytic degradation of CIP was nearly unchanged compared with the absence of scavengers. Our study indicates that CIP degradation is mainly caused by h+ and ˙OH, rather than e− driven reactions taking place on the surface of the photocatalyst.58 Therefore, it can be concluded that h+ and ˙OH are the main active species of Ag–TiO2 NPs in aqueous solution under visible light irradiation.
This is in line with our previous findings for CIP degradation under visible light in the presence of other similar catalysts, such as ZnO.59 Based on the experimental results, a possible mechanism of visible light photocatalytic degradation of CIP in the presence of the Ag–TiO2 NPs is illustrated in Scheme 2. As well known, TiO2 P25 is a mixture of anatase and rutile phase in a ratio of about 80/20,60,61 respectively. D. C. Hurum et al.62 reported that rutile phase, due to its slightly lower bandgap in comparison to anatase, can be active under visible light irradation. This fact explains why TiO2 P25 can degrade CIP and NFX under visible light irradiation. However, the rutile phase is present in a much lower amount than anatase and, therefore, the photocatalytic activity is low, and the measured bandgap for TiO2 P25 resembles more the one of anatase. The presence of Ag NPs on the TiO2 P25 enhances this photocatalytic activity upon visible light irradiation due to a better electron–hole pairs' separation. When the Ag–TiO2 NPs are irradiated with visible light, the rutile phase of TiO2 will be activated. The photogenerated electrons can be then transferred to Ag NPs and to the anatase phase. In particular, Ag clusters deposited on the TiO2 surface will act as electrons traps avoiding the recombination of electrons and holes and, therefore, enhancing the photocatalytic activity of TiO2. This explains why the mechanism is mainly hole-driven. Holes and ˙OH radicals which are produced by the reaction between the holes and the water molecules adsorbed on the photocatalyst's surface play an important role in the degradation of CIP to CO2 and H2O. The degradation of CIP due to O2˙− radicals is, instead, negligible based on our experiments with scavengers. Therefore, Ag contributes to the improvement of the photocatalytic activity of TiO2 under visible light, but the role played by the rutile phase in all the process seems to be essential and it was widely neglected in previous studies of TiO2 P25 based-systems under visible light irradiation.37 From the scavenger experiments, it can be estimated that ˙OH and h+ are the main active species in the photocatalytic degradation of CIP in the presence of Ag–TiO2 NPs in aqueous solution under visible light irradiation. In other reports about methylene blue degradation under visible light irradiation in the presence of Ag–TiO2 NPs, ˙OH radicals were found to be the main active species instead of holes and superoxide radicals.55 This stresses particularly the importance of the investigation of the photocatalytic mechanism for each specific pollutant/catalyst couple under certain selected conditions. However, one of the main results of this work concerns the importance of the rutile phase in the visible-light activation of TiO2 P25-based systems.
We believe that our manuscript provides important clarifications about the possible photocatalytic mechanism under visible light irradiation for Ag NPs decorated TiO2 P25 systems. Altogether, the prepared Ag–TiO2 NPs are a viable alternative for the degradation of fluoroquinolone-based antibiotics under visible light irradiation and, at the same time, for the inactivation of bacteria in water. It is foreseen that the Ag–TiO2 NPs will find practical utilisation and application in water treatment, especially in that of hospital wastewater, where the removal of pharmaceuticals and the disinfection from bacteria is a desirable final aim.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ra10403e |
‡ Current address: International Iberian Nanotechnology Laboratory, Avenida Mestre José Veiga s/n, 4715-330 Braga, Portugal. |
This journal is © The Royal Society of Chemistry 2021 |