Sang Gi Honga,
Eunmi Im‡
b,
Da In Kima,
Eun Jin Jeongb,
Jongbok Kimcd,
Geon Dae Moon*b and
Dong Choon Hyun*a
aDepartment of Polymer Science and Engineering, School of Applied Chemical Engineering, Polymeric Nano-materials Laboratory, Kyungpook National University, Daegu 41566, South Korea. E-mail: dong.hyun@knu.ac.kr
bDongnam Division, Korea Institute of Industrial Technology, Busan 46938, Korea. E-mail: gmoon@kitech.re.kr
cDepartment of Materials Science and Engineering, Kumoh National Institute of Technology, Gumi, Gyeongbuk 39177, Korea
dDepartment of Energy Engineering Convergence, Kumoh National Institute of Technology, Gumi 39177, Korea
First published on 13th April 2021
This work introduces the fabrication of a magnetic polymer bowl for enhanced catalytic activity and recyclability, which involves the synthesis of silica-coated Fe3O4 magnetic clusters, seeded dispersion polymerization using the magnetic clusters, and transformation into a bowl-like structure via a phase separation route. The additional treatment with tannic acid (TA) on the bowls allows the in situ formation of silver nanoparticles (AgNPs) on their surfaces. The openness and larger surface area of the bowls, as compared with those of other structured particles, such as spheres and flowers, enable a considerably higher immobilization of AgNPs, thus leading to an excellent catalytic reduction for 4-nitrophenol (4-NP), methylene blue (MB), and rhodamine B. Furthermore, the strong magnetic response originating from the magnetic clusters inside the bowls endows a good magnetic recovery and an excellent reusability for the repeated reduction of the organic dyes without loss of catalytic activity.
Among several techniques developed for the removal of organic dyes, chemical approaches using nanomaterial catalysts, which can convert organic dyes into non-/less toxic or useful products through change in their molecular structures, have recently gained considerable attention owing to its high efficiency, low cost, and simple setups.8,9 For example, 4-NP can be reduced to 4-aminophenol (4-AP) in the presence of catalysts and reductants, which is a useful compound in pharmaceutical industry.10 Similarly, rhodamine B and MB can be reduced to colorless compounds (leuco rhodamine B and leuco MB) with the use of proper catalysts in the presence of NaBH4.11,12 When catalytic activity and chemical/physical stability are concerned, noble metal nanoparticles (NPs), including platinum (Pt), silver (Ag), and gold (Au) have been considered as the optimal catalysts.2,13,14 However, the poor colloidal stability, originating from their high surface area, and difficulty in separation cause the decrease of active sites and catalytic performance for the reduction of organic dyes.15 In addressing this issue, the use of various supports to deposit noble metal NPs on their surfaces has been reported.16 Among them, polystyrene (PS) particles have shown numerous advantages as a catalytic support material, such as their simple and large scalable synthesis, monodispersity and controllability in size and shape, good dispersion in various media, and easy surface modification.17–20 Because most of previously reported studies have used, however, solid PS particles with a relatively low surface area,20–26 it is difficult to increase the loading amount of noble metal NPs. Alternatively, numerous studies have reported the fabrication of PS particles with hollow structures to provide large surface areas.27 However, the closed shells in most of the hollow particles allow the deposition of noble metal NPs only on the outer surfaces, not exhibiting a higher deposition of noble metal NPs compared with solid PS particles. Furthermore, their limited recovery from reaction system by centrifugation or filtration causes a poor reusability during cycles of catalytic process, consequently hindering their practical applications to the treatment of toxic organic dyes.
In this study, we demonstrate the fabrication of a magnetic polymer bowl for the enhanced catalytic activity and recyclability. The magnetic polymer bowl is prepared through synthesis of silica-coated Fe3O4 magnetic clusters, their surface treatment with vinyl group, and seeded dispersion polymerization under the use of the magnetic clusters, followed by phase separation for the transformation into bowl-like structure (Scheme 1). The additional treatment with tannic acid (TA) on the bowls allows the in situ formation of AgNPs on their surfaces. The openness and larger surface area of the bowls, as compared with those of other structured-particles such as spheres and flowers, enable a considerably higher immobilization of AgNPs, leading to an excellent catalytic reduction for 4-NP, rhodamine B, and MB. Furthermore, the strong magnetic response arising from the magnetic clusters inside the bowls endows a good magnetic recovery and an excellent reusability, achieving twenty consecutive reduction of the dye molecules with no loss in catalytic activity.
Scheme 1 Schematic illustration of the procedure for fabricating magnetic polymer bowl with highly immobilized AgNPs. |
The surfaces of the magnetic clusters were silica-coated for enhancing their chemical stability and acid resistance, as well as for conducting further chemical reactions to make magnetic polymer particles. In this study, the Stöber method, which has been mainly employed for silica coating,32 was used. Fig. 2A shows a TEM image of the magnetic clusters obtained after the treatment using the Stöber method, demonstrating the formation of spherical particles that consist of single magnetic cores and silica shells with uniform thickness. The silica-coated magnetic clusters had a mean diameter of 401 ± 21 nm. Using this result and the diameter of the magnetic clusters in Fig. 1A, the coating layer thickness was calculated to be about 73 nm, which was also confirmed in the inset image. The XRD pattern of the silica-coated sample was the same as that of the magnetic clusters in Fig. 1C (Fig. S2A, ESI†), suggesting that the coating did not affect the crystalline structure of the magnetic cluster cores. Consequently, the silica-coated particles still retained a strong magnetic response driven by the magnetic cores (Fig. S2B and C†).
These silica-coated particles were employed as seeds for preparing magnetic polymer particles. When we carried out the polymerization using the particles in Fig. 2A as seeds, the PS particles separated from the magnetic seeds were made (Fig. S3, ESI†), indicating no interaction between both of the two components. To improve the interaction, the silica-coated particles were modified with MPS to induce the formation of vinyl groups on their surfaces. We controlled the grafting density of MPS by varying its treatment conditions, such as the volume of MPS and treatment time, followed by determining the density value (QMPS, μmol m−2) using UV-vis spectrometry (see ESI†). When the silica-coated magnetic clusters were treated with 1 mL of MPS for 24 h, the calculated QMPS was 1 μmol m−2. The incubation with 2 mL of MPS for 5 days increased the value of QMPS to 4.5 μmol m−2. Fig. 2B shows a TEM image of the particles made by the polymerization at 70 °C for 6 h under the use of the MPS-treated seeds with QMPS of 1 μmol m−2, which demonstrates the formation of flower-like particles, consisting of PS nodules attached to one seed. This result was because the MPS treatment promoted favorable interactions between the seed and polymer species, leading to a covalent grafting of PS chains on the surfaces of the seeds.33 As shown in Fig. S4A (ESI†), all the particles exhibited the flower-like structure, suggesting that the large-scale preparation of flower-like particles is possible. The mean diameter of each nodule was measured to be 355 ± 12 nm, and the number of PS nodules per seed was 8 on average. However, the use of the seeds with QMPS of 4.5 μmol m−2 formed the spherical particles with MPS-treated seed cores and PS shells (Fig. 2C). The mean diameter of the spheres was 752 ± 21 nm. For all the spheres, encapsulation of the seeds was observed, as shown in Fig. S4B.† This structural change can be explained using the difference in QMPS value. When QMPS is high, the increased affinity of PS to the functionalized seed surfaces allows the collapsing of growing polymer chains or the coalescence of freshly nucleated polymer domains, eventually forming a polymer shell fully coating the seeds.34 For low QMPS, however, the high interfacial energy between the seed and PS blocks the spreading of the PS chains on the surfaces of the seeds or the merging of the polymer domains, consequently generating the polymer nodules around the seeds.33
The spherical particles in Fig. 2C were additionally treated at 70 °C for 2 h together with decane, EHMA, and AIBN for their transformation into bowl-like structure. At the elevated temperature, the decane molecules tend to absorb into the polymer phase. Due to the phase separation between the absorbed molecules and polymer phase, the small-sized decane domains starts to form within the polymer, followed by merging into single-phased interiors over time. The interior voids and surface holes are created during the removal of decane.19 Fig. S5 (ESI†) shows an SEM image of the particles obtained through the thermal treatment and washing in ethanol and isoamyl alcohol, demonstrating that the core–shell spheres were successfully transformed into bowl-like particles with hollow voids and large surface openings. The formation of the voids and open holes could be more clearly observed in the TEM image of Fig. 2D. Furthermore, it turned out that each seed with a magnetic cluster and a silica shell was still encapsulated in the bowl-like particle after the transformation, as shown in the inset TEM image, indicating that a sequence of treatments, such as MPS modification, polymerization, and transformation, did not affect the structure of the seed. Maintaining the seed structure rendered the polymer bowls magnetically responsive (Fig. S6, ESI†), with a saturation magnetization of 51.2 emu g−1 (Fig. S1†) that was much higher than the result reported in a previous study.12 Similar results were observed in the flower-like and spherical particles, as shown in the insets in Fig. 2B and C, along with Fig. S6.†
To provide a catalytic property to the magnetic polymer particles, we immobilized AgNPs on the polymer particles owing to their low cost, unique reactivity and selectivity, and good stability, as well as recyclability in catalytic reactions.35 Before the immobilization, Fe3+ and TA were consecutively deposited on the magnetic polymer particles. When Fe3+ was injected into the dispersion of the magnetic polymer particles, the cation was adsorbed on the negatively charged particles, which led to the change in their zeta potential (Fig. S7, ESI†). Subsequently, the addition of TA, which is a green reducing agent, induced the chelation of the molecules with the Fe3+ layer. The repetition of this process formed a highly stable coating of TA–Fe with good uniformity on the surfaces of the magnetic polymer particles, which could provide a homogeneous reduction environment on the highly curved surfaces.36 When Ag(NH3)2+ was injected into the dispersion of the magnetic polymer particles treated with Fe3+ and TA, the in situ reduction of the ion occurred on the magnetic polymer particles because of the catechol groups in TA molecules deposited on the particles.
Fig. 3A shows an SEM image of the resultant sample after the repeated deposition of Fe3+ and TA on the particles of Fig. S5,† followed by the reduction process. The particles exhibited the uniform distribution without aggregation and the bowl-like structure with hollow interior and large surface opening, which suggest no structural change after a series of processes involving the deposition and reduction. The TEM image in the inset shows the formation of the small spherical NPs on the surface of the magnetic polymer bowl. They exhibited a good uniformity in size, with a mean diameter of 6 nm. To investigate the elements present in the bowls, EDS analysis was carried out. C, O, Fe, Si, and Ag were observed (Fig. S8, ESI†). The existence of these elements was also confirmed using XPS measurement, as shown in Fig. S9 (ESI†), which suggests the in situ formation of AgNPs. These AgNP-immobilized, magnetic polymer bowl still retained a high magnetization (Fig. S1†), which suggests that their rapid recovery from reaction system is achievable using a magnet. Similar results were observed for the magnetic polymer flowers and spheres. They could immobilize AgNPs on their surfaces without any structural change, as shown in Fig. 3B and C. Furthermore, the AgNP-immobilized, non-magnetic polymer spheres were prepared using PS particles with a mean diameter of 750 ± 18 nm (Fig. 3D).
We examined the catalytic performance of these particles for the reduction of 4-NP. After the AgNP-immobilized, magnetic polymer spheres in Fig. 3C were introduced into an aqueous system containing 4-NP and NaBH4, the temporal change of UV-vis absorbance spectra at 25 °C for the system was monitored (Fig. 4A). While the intensity located at 400 nm (I400) decreased over time, a new peak started to appear at 300 nm and its intensity increased gradually, indicating that 4-AP formed as a resultant product from the reduction of 4-NP.36 A similar reduction behavior was observed in the AgNP-attached polymer spheres (Fig. 4B). In contrast, there was no change in I400 in the absence of the AgNP-attached, magnetic polymer spheres (Fig. S10A, ESI†). The addition of the magnetic polymer spheres without immobilized AgNPs exhibited no change in I400, either (Fig. S10B†). These results indicate that the reduction of 4-NP was induced by the attached AgNPs, which can assist the electron transfer from BH4− to the dye molecules adsorbed on the NPs.12 Interestingly, the reduction behavior of 4-NP was more enhanced under the use of the magnetic polymer flowers and bowls with immobilized AgNPs (Fig. 4C and D). The I400 values for the flowers and bowls decreased by 67 and 85% in the initial 10 min, whereas the magnetic polymer spheres with immobilized AgNPs exhibited a decrease in I400 by 46% during the same period. Assuming that each magnetic polymer particle with immobilized AgNPs worked as each catalytic center, we could determine the turnover frequency (TOF), which quantifies the specific activity of a catalytic center for a reaction under defined conditions,37 of the AgNP-immobilized magnetic polymer particles (see ESI†). The TOF value for the magnetic polymer bowl with attached AgNPs was calculated to be 3.01 × 1011 min−1, which was larger than those for the other magnetic particles (9.11 × 1010 min−1 for the magnetic polymer sphere and 1.61 × 1011 min−1 for the magnetic polymer flower). This result indicates that the magnetic polymer bowl-based system had more enhanced catalytic activity for the reduction of 4NP than the other particles.
To further study the catalytic performance of the AgNP-attached particles in Fig. 3, we also examined the reduction behaviors at 25 °C of rhodmaine B and MB under the use of these particles. As shown in Fig. 5, all the samples exhibited a gradual decrease in I554 over time, indicating the reduction of rhodamine B.6,12 However, the reduction rate differed in each sample. As in the case of the 4-NP, the fastest reduction was observed in the bowl sample, with a decrease in I554 by 74%, followed by the magnetic polymer flower (52% decrease) after the initial 10 min. Conversely, the magnetic and non-magnetic polymer spheres exhibited very slow reduction reactions, with I554 decrease by 34%. The catalytic reduction order was also same in the case of MB (Fig. 6).
Additionally, the reduction of these organic dyes was examined at different temperatures (4 and 37 °C), as shown in Fig. S11–S16 (ESI†). In all the reduction tests, because the concentration of NaBH4 was one hundred times higher than that of each dye, it could be assumed that the reduction of the dye molecules was not affected by the change in the concentration of NaBH4 during the whole reactions. Under this assumption, the first-order reaction kinetics could be used to understand the reduction of the dyes. Based on the linear relation between −ln(It/I0), where It and I0 are the absorbance peak intensities at time t and zero, and the time for each reaction (Fig. S17–S19, ESI†), the reaction rate constant (k) for each reduction system was evaluated. From the obtained value of k, the activation energy (Ea) for the reduction reaction of each dye could be estimated using the Arrhenius equation, i.e., lnk = lnA − Ea/RT, where A and R denote the pre-exponential factor and ideal gas constant, respectively. For 4-NP, the k values at 4, 25, and 37 °C for the magnetic polymer bowls were 0.082, 0.202, and 0.319 min−1, which were larger than those at the corresponding temperatures for the other particles (Table 1). Furthermore, the k value at 25 °C was higher than the results reported in previous studies.38–41 The high k value for the magnetic polymer bowls was also observed in rhodamine B and MB. Conversely, the Ea values for the reduction of each dye were similar, irrespective of the type of AgNP-immobilized particles, which suggests that the reduction mechanism of each dye was the same for all the particle types. It is well known that the catalytic reduction of dye molecules, including 4-NP, rhodamine B, and MB, in the presence of NaBH4 takes place on the surface of noble metal nanocatalysts.42–44 BH4− ions, which are produced from ionization of NaBH4, are adsorbed on the surface of the nanocatalysts, forming surface-bound hydrogen as metal hydride. At the same time, the dye molecules are also attached on the surface of the nanocatalysts. The hydrogen interacts with the adsorbed dye molecules, causing their reduction to 4-AP, leuco methylene blue, and leuco rhodamine B.9,42,45 As shown in Table 1, the Ea values for all the organic dyes were in the range of 8–40 kJ mol−1, corresponding to the result of surface catalyzed reactions,46 which suggests that surface catalysis induced the reduction of the dye molecules.
Dye | Particle | k (min−1) | Ea (kJ mol−1) | ||
---|---|---|---|---|---|
4 °C | 25 °C | 37 °C | |||
4-NP | Non-magnetic sphere | 0.025 | 0.062 | 0.098 | 29.6 |
Magnetic sphere | 0.024 | 0.061 | 0.101 | 30.2 | |
Magnetic flower | 0.043 | 0.108 | 0.179 | 30.5 | |
Magnetic bowl | 0.082 | 0.202 | 0.319 | 29.2 | |
Rhodamine B | Non-magnetic sphere | 0.014 | 0.042 | 0.073 | 35.8 |
Magnetic sphere | 0.014 | 0.042 | 0.073 | 35.8 | |
Magnetic flower | 0.023 | 0.073 | 0.130 | 37.4 | |
Magnetic bowl | 0.046 | 0.142 | 0.244 | 36.3 | |
MB | Non-magnetic sphere | 0.030 | 0.073 | 0.115 | 29.1 |
Magnetic sphere | 0.030 | 0.070 | 0.112 | 28.5 | |
Magnetic flower | 0.051 | 0.127 | 0.199 | 29.0 | |
Magnetic bowl | 0.096 | 0.231 | 0.366 | 28.9 |
To understand the higher k value in the magnetic polymer bowls for all the dyes, we calculated the volume (V) and surface area (S) of a magnetic polymer bowl, followed by comparing the values with those of the other-structured particles. For the calculation of V and S of each type of magnetic polymer particle, simple models were used, as illustrated in Scheme 2. For the magnetic polymer sphere, a simple model, consisting of the silica-coated Fe3O4 seed and surrounding polymer, was considered (Scheme 2A). The V and S of a magnetic polymer sphere can be expressed as V = (4/3)πRouter3 and S = 4πRouter2, where Router denotes the outer radius of the sphere, which could be determined using the TEM images of the magnetic polymer spheres. For the magnetic polymer flower, V can be expressed as V = (4/3)πRseed3 + (4/3)πRnodule3Nnodule, where Rseed, Rnodule, and Nnodule denote the radius of the magnetic seed, radius of the polymer nodule, and number of polymer nodule attached to the magnetic seed, respectively (Scheme 2B). Assuming that the surface of the silica-coated magnetic core is fully covered with polymer nodules, the S of a magnetic flower can be expressed as S = 4πRnodule2Nnodule. The V and S of the flower could be estimated from the Rseed, Rnodule, and Nnodule values obtained using the TEM images of the magnetic polymer flowers. In the case of the magnetic polymer bowl, V can be expressed as V = (1/3)πRpolymer3(2 + 3cosθpolymer − cos3θpolymer) − (1/3)πRvoid3(2 − cosθvoid + cos3θvoid),47 where Rpolymer and Rvoid denote the radii of the magnetic core-encapsulated polymer and void phases, respectively, and θpolymer and θvoid are the angles opposite to the line segment connecting from the intersection of the two phases to center of each phase (Scheme 2C). Assuming that there is no loss of polymer chains during the transformation into bowl-like particles, its volume is the same as that of a magnetic polymer sphere. The S of a magnetic polymer bowl can be expressed as S = 4πRpolymer2 − 2πRpolymer2(1 − cosθpolymer) + 2πRvoid2(1 − cosθvoid).19 The additional relations among Rpolymer, Rvoid, θpolymer, and θvoid are given as DH = 2Rpolymersinθpolymer = 2Rvoidsinθvoid by taking the diameter of the single opening (DH) on the surface of the bowl into consideration. The value of θpolymer could be theoretically calculated using Rpolymer and DH, which were determined from the TEM images for the magnetic polymer bowls. Taking the V of the magnetic polymer sphere together with DH, the values of Rvoid and θvoid could be estimated. Using the obtained θpolymer, θvoid, Rpolymer, and Rvoid values, we calculated S of the magnetic polymer bowl. Fig. S20 (ESI†) shows the calculated V for each type of magnetic polymer particle. The values of V for the non-magnetic polymer sphere and magnetic polymer particles (sphere, flower, and bowl) were very similar to each other, whereas the S values were different. As shown in Fig. 7A, the magnetic polymer bowl exhibited the largest S value (5.86 × 106 nm2), followed by the magnetic flower and both the spheres.
Scheme 2 Schematic illustration of magnetic polymer particles for calculating their volumes and surface areas: (A) sphere, (B) flower, and (C) bowl. |
Fig. 7 (A) Surface areas (S) for the different types of magnetic polymer particles. (B) Numbers of immobilized AgNPs per magnetic polymer particle (XAg). |
Furthermore, we evaluated the number of AgNPs immobilized on one magnetic polymer particle (XAg) via ICP-MS analysis (see ESI†). The XAg for all the polymer particles with attached AgNPs is shown in Fig. 7B. The value of XAg of the magnetic polymer bowl was 8.2 × 103, which was larger than those of the other particles. This result indicates that the bowls were able to more effectively immobilize the AgNPs on their surfaces. To correlate the obtained S and XAg values, the normalization for S and XAg was conducted. As shown in Fig. S21 (ESI†), the normalized values in S for the magnetic polymer particles were consistent of those in XAg for the corresponding particles, which indicates that the openness of the bowls allowed the deposition of AgNPs on both their outer and inner surfaces. Moreover, the values were in good agreement with the normalized results in k, which were obtained by dividing k at each temperature for each type of magnetic polymer particles by that for the non-magnetic polymer spheres (Table 1). This similarity suggests that the larger surface area and openness of the magnetic polymer bowls led to the greater immobilization of AgNPs, which functioned as the reactive sites, thus inducing the enhanced catalytic activity and higher k value.
We also performed the reusability test of the magnetic polymer particles with immobilized AgNPs by examining their catalytic performances during repeated cycles of rhodamine B reduction. Upon the application of a magnet, the particles could be separated in 3 min from the reaction solution after each cycle of the reduction reaction and were then reused as catalysts. Fig. 8A shows the extent of conversion (α) of the organic dye, which is given as α = (I0 − It)/I0, after the reaction for 30 min at 25 °C. The AgNP-attached, magnetic polymer bowls exhibited the highest α (over 0.98), and the values were similar for twenty cycles. Similarly, the high k value of the bowls was maintained even after the repeated reduction reactions (Fig. 8B). These results demonstrate the excellent stability and reusability of the magnetic polymer bowls with immobilized AgNPs, making them useful as a recoverable and efficient system for enhanced and repeated reduction of toxic organic dyes.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra00453k |
‡ These authors contributed equally to the preparation of this paper. |