Jing Donga,
Wenjian Fangb,
Weiwei Xiac,
Qihong Luc and
Xianghua Zeng*bc
aCollege of Chemistry and Chemical Engineering, Yangzhou University, Yangzhou 225002, P. R. China
bCollege of Electrical, Energy and Power Engineering, Yangzhou University, Yangzhou 225127, P. R. China. E-mail: xhzeng@yzu.edu.cn
cCollege of Physics Science and Technology & Institute of Optoelectronic Technology, Yangzhou University, Yangzhou 225002, P. R. China
First published on 18th June 2021
Hydrogen evolution from water using solar energy is regarded as a most promising process, thus, exploring efficient photocatalysts for water splitting is highly desirable. To avoid the rapid recombination of photogenerated electrons and holes in CdZnS semiconductors, ZnxCd1−xS/ZnS composites were synthesized via a one-step hydrothermal method and then annealed at 400 °C for 60 min under argon flow. ZnxCd1−xS/ZnS composites are composed of ZnS nanosheets decorated with ZnxCd1−xS nanorods, and TEM and UV-vis absorption spectra confirm the formation of the heterostructure between ZnxCd1−xS nanorods and ZnS nanosheets. Because of the well-matched band alignment, stronger optical absorption and larger carrier density, Zn0.2Cd0.8S/ZnS has the highest hydrogen production, with a photocatalytic hydrogen production rate up to 16.7 mmol g−1 h−1 under visible light irradiation. Moreover, the photocatalyst also exhibits high stability and good reusability for hydrogen production reaction. The facile and efficient approach for ZnS based heterostructures could be extended to other metal compound materials.
Ternary ZnCdS nanomaterials were regarded as a promising substitute for noble-metal co-catalysts in photocatalytic reactions because of their tunable band gap energy and lattice constant between 0.331 (〈100〉 of ZnS) and 0.359 nm (<〈100〉 of CdS) in comparison with ZnS or CdS materials.2–6 Recently some studies on ZnCdS- related photocatalytic hydrogen reactions have been reported. Such as, Jin et al.7 reported that ZnCdS catalysts with a (Zn + Cd):S molar ratio of 1:3.5 has much higher photocatalytic activity and exhibited an excellent stability after six cycles. And the H2 production of (CdS–ZnS)–TiO2 supported photocatalytic system was studied by Tambwekar et al.8 The hydrogen evolution rate of ZnCdS–CdS heterostructure was obtained from 25.46 to 72.82 and 52.82 μmol h−1, and the value increased to 192.28 μmol h−1 after the adoption of VS2 to the heterostructure surface.9 GQDs/ZnCdS/PdS exhibited a H2 evolution rate of 517 μmol h−1, which is 15, 7 and 1.7 times higher than that of pure ZnCdS, GQDs/ZnCdS, and ZnCdS/PdS, respectively.10 α-Fe2O3/Zn0.4Cd0.6S heterostructure has visible light photocatalytic H2 production of 536.8 μmol h−1.11 The ZnCdS–CH solid solution without noble metal loading achieved a superior photocatalytic H2 activity rate of 0.971 mmol h−1 under visible light irradiation (λ ≥ 420 nm), which exceeds those of coprecipitated Zn0.5Cd0.5S samples by more than 13 times.12 The hydrogen production rate of Fe1−xPtx-ZnCdS NPs had a significant enhancement over the pure ZnCdS (740 μmol g−1 h−1). The hydrogen production activity of ZnCdS–NiCoP composite catalyst was improved greatly, which reached 5.2 times that of pure ZnCdS.13 The highest hydrogen production rate of 2.265 mmol g−1 h−1 was achieved by the 0.5 wt% Fe0.3Pt0.7–ZnCdS nanocomposites, which was even better than that of 0.5 wt% Pt–ZnCdS (1.626 mmol g−1 h−1) under the same condition.14
The photocatalytic H2 evolution rate of Zn0.3Cd0.7S nanorods was improved from 517.4 to 3310.1 μmol g−1 h−1 by loading a suitable amount of Ni3C NPs as co-catalyst under visible light irradiation.15 Hollow Zn0.6Cd0.4S cage material exhibited the highest hydrogen production rate of 5.68 mmol h−1 g−1 under cocatalyst-free and visible-light irradiation conditions.16 The addition of NiB greatly improved the photocatalytic performance of CdZnS, and the hydrogen production of NiB/CdZnS catalysts reached 8.137 mmol g−1 h−1, which is 17 times that of pure CdZnS.17 A typical “type II” band alignment forms at Zn0.5Cd0.5S hybrided with carbon materials lead to the improved H2 generation rate of 10.8 mmol g−1 h−1, exceeding the Zn0.5Cd0.5S nanosheets (6.4 mmol g−1 h−1) and QDs (3.4 mmol g−1 h−1).18 A controlled ZnCdS QDs developed by a simple ZIF-8 templating method exhibited significantly enhanced photocatalysis performance with a H2 production rate of 3.70 mmol h−1 g−1 (Zn0.5Cd0.5S QDs),19 and the highest hydrogen production rate of Zn0.5Cd0.5S/dodecahedron ZIF-67 composite reached 23.264 mmol g−1 h−1 under visible light irradiation,20 which was explained as the matched valence band position for ZIF-67 and ZCS and the exposure of rich active sites. The WO3/ZnCdS compound catalysts showed the hydrogen production activity of the 35 wt% WO3/ZnCdS to 98.68 μmol mg−1, about 9.6 times that of pure ZnCdS (10.28 μmol mg−1).21
Although many efforts have been done to develop efficient photocatalytic systems and photocatalysts by using ZnCdS materials and their composites, it is still an urgent task to develop low-cost co-catalysts for advancing photocatalytic H2 production. In this paper, simple hydrothermal and annealing reaction methods were developed for preparation of pure ZnS nanosheets, CdS nanorods and ZnxCd1−xS/ZnS composites. The photocatalytic hydrogen production rate of Zn0.2Cd0.8S/ZnS (#3) up to 16.7 mmol g−1 h−1 has been obtained under visible light irradiation with a good stability. This value is larger than the reported pure ZnxCd1−xS/ZnS composites. Furthermore, the preparation method is simple. The outstanding photocatalytic performance benefited from the efficient charge transfer between ZnCdS nanorods and ZnS nanosheets in the ZnxCd1−xS/ZnS heterojunctions, as well as more active sites on the surface of nanosheets. This study will be helpful to obtain catalysts for photocatalytic H2 production based on low-priced metal composite materials.
The PEC analysis was carried out on Zahner CIMPS electrochemical workstation (Germany) in a quartz cell, using a three-electrode cell with a Pt wire as the counter electrode, Ag/AgCl electrode as the reference electrode and FTO glass covered with photocatalyst as the working electrode. A 300 W Xe lamp (CEL-HXF 300, Beijing Au-light, China) was employed as an incident light source to study the PEC response of the samples, and Na2SO4 (0.2 M) solution was used as the electrolyte.
Fig. 1 Scheme of photocatalytic reactor and closed gas circulation and evacuation system made of Pyrex glass. |
Fig. 2 (a) and (b) XRD patterns of samples ZnS (#1), ZnxCd1−xS/ZnS (#2, #3) and CdS (#4); (c) EDX spectrum for sample #3. |
d | (h k l) | 2θ | |
---|---|---|---|
#2 | 3.5005 | (100) | 25.424 |
3.2940 | (002) | 27.047 | |
3.0912 | (101) | 28.858 | |
#3 | 3.5239 | (100) | 25.252 |
3.3105 | (002) | 26.910 | |
3.1107 | (101) | 28.674 |
The atomic weight percentages of the constituents are given in Table 2, we find that the metal element Zn is dominated in sample #3, and the compositional percentages of (Zn2+ + Cd2+) and S2− are in the required stoichiometric ratio, but larger than 1. So, there are a lots of sulfur vacancies in the prepared samples.
Element | Atomic percentage % |
---|---|
S | 40.15 |
Zn | 54.83 |
Cd | 5.00 |
The morphologies of samples #1, #3 and #4 were investigated with SEM images as shown in Fig. 3. From Fig. 3a, sample #1 is composed with nanosheets, each nanosheet has a thickness of about 50 nm (inset of Fig. 3a), and sample #4 is composed with nanorods, each individual nanorod has a diameter of several tens nm and length of several hundred nm (Fig. 3b). Low- and high-magnification images of sample #3 were displayed in Fig. 3c and d, which show that after replacing Zn precursor with Cd, the products are mainly composed with nanosheets with some nanorods sparsely growing on the surface of ZnS nanosheets. Sample #2 has the same morphology as sample #3, but it is thicker and narrower than sample #3.
TEM and HRTEM measurements were carried out to investigate the microstructure features, and HAADF-STEM to determine the elements distribution. TEM images of selected ZnxCd1−xS/ZnS are displayed in Fig. 4a, the nanorods with a diameter of ∼20 nm were grown on the nanosheets, which is consistent with the result of SEM. Furthermore, from the HRTEM image (Fig. 4b), one can find that the well-resolved lattice fringes with separations of 3.53 and 3.31 Å matched well with the interplanar spacing of (100) and (002) of Zn0.2Cd0.8S with a high crystallinity, indicating that the Zn0.2Cd0.8S nanorods grows along the [001] direction. At the same time, the lattice spacing of 3.13 Å in the nanosheet matched well with the (002) plane of hexagonal ZnS. The result is in good agreement with XRD. From elemental mappings in Fig. 4c–f, it is found that Zn and S were well-distributed, while Cd mainly gathered in nanorod area, the results confirm that #2 and #3 were composed of both ZnS nanosheets and ZnxCd1−xS nanorods, and ZnxCd1−xS nanorods were sparsely distributed on the surface of ZnS nanosheets.
Therefore, from the XRD patterns, SEM and TEM images show that samples #2 and #3 were composed with ZnS/ZnxCd1−xS heterostructures with ZnS nanosheets decorated with ZnxCd1−xS nanorods.
The PL spectra were carried out to study the properties of electrons' recombination light emission. As displayed in Fig. 5a, a wide peak from 400 to 700 nm was observed for all the samples, while ZnS (sample #1) has the strongest PL intensity, which was ascribed to the sulfur-related, zinc-related vacancies and the surface states.26,27 A decrease in the fluorescence intensity in samples #2 and #3 implies the suppressed recombination of photogenic electron–hole pairs upon attaching ZnxCd1−xS nanorods on ZnS nanosheets, and an increased photogenerated electron–hole separation, and the shift of peak position probably attributed to the transition at the interface.
UV-vis-NIR absorption spectra (Fig. 5b) reveal that samples #1 and #4 have only a single typical absorption edge, while two absorption edges can be easily found in samples #2 and #3, one at ∼358 nm is ascribed to ZnS, the other at ∼500 for sample #2 and ∼525 nm for sample #3 can be attributed to the intrinsic bandgap absorption of ZnxCd1−xS. The observed two absorption edges in samples #2 and #3 reveal the formation of the ZnxCd1−xS/ZnS heterostructures. Sample #3 has a stronger absorption and bigger absorption edge than sample #2. Then, the band gap energy is obtained as 3.46, 2.48, 2.35 and 2.19 eV for samples #1–#4, respectively.
The hollow porous structures of the as-prepared samples were elucidated by nitrogen adsorption/desorption measurements to obtain their BET surface areas. As shown in Fig. 5c, the BET surface area was calculated to be 149.3 m2 g−1 for pure ZnS nanosheets (#1), and 103.2, 82.3 and 20.9 m2 g−1 for #2, #3 and #4, respectively. From the results, one can find that pure CdS nanorods possess a low BET surface area, and sample #3 has larger BET surface than sample #2, which is favorable to adsorb molecules.
Fig. 5 (a) PL spectra, (b) UV-vis absorption spectra and (c) BET surface areas for the prepared samples ZnS (#1), ZnxCd1−xS (#2, #3) and CdS (#4). |
XPS measurements were used to investigate the surface composition of the four samples, the binding energies have been calibrated using the carbon C 1s peak (285.0 eV) as reference. Zn 2p spectra exhibited two peaks at ∼1020.9 eV and 1043.8 eV, which were assigned to Zn 2p3/2 and 2p1/2 of Zn2+, as shown in Fig. 6a. In comparison with sample #1, the Zn 2p binding energy in ZnxCd1-xS/ZnS heterostructures (#2, #3) has a slightly shift to higher energy, indicating the decreased electron density around Zn atoms.28 The Zn 2p3/2 core level spectra can be deconvolved into two peaks, as shown in Fig. 6b, where the lower one is ascribed to zinc in the lattice, while the higher one was related to the Zn2+ in the sulfur deficient regions.29 The relative intensity ratios between the higher one and total zinc are equal to 0.298, 0.280 and 0.285 for sample #1, #2 and #3, respectively. That means, many sulfur vacancies exist in sample #2 and #3, and the concentration is approximate, consistent with the EDX results. The Cd 3d XPS spectra are shown in Fig. 6c, in which two peaks at 404.4 eV and 411.1 eV correspond to Cd 3d5/2 and 3d3/2, respectively, and there is no obvious peak shift between pure CdS nanorods and ZnxCd1-vxS/ZnS heterostructures. For S 2p, the peaks at about 161.0 eV and 162.2 eV are belong to S 2p3/2 and S 2p1/2, as shown in Fig. 6d. With the introduction of Cd, the peaks of S shift to a lower binding energy, implying that the introduction of Cd atoms leads to the formation of ZnxCd1−xS. The above XPS analyses demonstrated that the electron transformation from Zn and Cd to S in ZnxCd1−xS/ZnS heterostructures can increase electron density of active sites and beneficial to the various reactivity.30,31
The apparent quantum efficiency was measured using the 300 W xenon lamp with a 420 nm band pass filters and calculated according to eqn (1):
(1) |
The photocatalytic H2 production was carried out under visible light irradiation (with a 420 nm cut filter) for samples ZnS, CdS and ZnxCd1−xS/ZnS, as shown in Fig. 7a. From Fig. 7a, we found that pure ZnS nanosheets exhibit no photocatalytic activity due to the poor visible light absorbability, while ZnS nanosheets decorated with ZnxCd1−xS nanorods reveal an enhanced photocatalytic activity. Sample Zn0.3Cd0.7S/ZnS has a hydrogen production rate of 9.2 mmol g−1 h−1, while Zn0.2Cd0.8S/ZnS (#3) achieved a H2 production rate up to 16.7 mmol g−1 h−1 with an apparent quantum efficiency of 10% at 420 nm, approximately 1.5 times of the former. The value is nearly three times of pure CdS nanorods (5.9 mmol h−1 g−1).32 This result is larger than recently reported 10.8 mmol g−1 h−1 with Zn0.5Cd0.5S hybrided with carbon materials as catalysts,18 but smaller than the value of 23.264 mmol g−1 h−1 with Zn0.5Cd0.5S/dodecahedron ZIF-67 composite.20 Moreover, different from the reported severe photocorrosion happened in CdS materials,33–35 the as-prepared Zn0.2Cd0.8S/ZnS heterostructures have a relatively stable H2 reproduction with seven consecutive cycles (Fig. 7b), and the initial low rate of hydrogen production was mainly attributed to the activation process of the catalyst.
EIS measurements was carried out to understand the charge transfer process and the electron–hole separation efficiency occurring at the interface between the photoelectrode and electrolyte, as presented in Fig. 7c, the semicircle in the Nyquist plot of each sample corresponds to the parallel combination of Rct and CPE1.36 The resultant values for the components of the EEC model corresponding to the best fit are presented in Table 3. The smaller diameter corresponds to the lower charge transfer resistance. One can find that sample #3 has smaller charge transfer resistance.
Sample | #4 | #1 | #2 | #3 |
Rs (kΩ) | 22.31 | 25.32 | 25.83 | 23.16 |
Rct (MΩ) | 150.8 | 164.6 | 38.73 | 30.50 |
Mott–Schottky (M–S) plots were explored to determine the flatband potential (Vfb) for the four sample, as depicted in Fig. 7d. All curves show positive slopes, corroborating the n-type characteristics. M–S plots can also be used to estimate the electron carrier concentration using the following equation.37
(2) |
In consideration of band gap energy and the conduction band potential versus Ag/AgCl electrode, the energy band alignment can be obtained for sample #3, as shown in Fig. 8. The figure shows that it is type-II heterojunction for Zn0.2Cd0.8S/ZnS heterostructure. For Zn0.2Cd0.8S/ZnS heterostructure, under visible-light irradiation (λ > 420 nm), electrons will be excited from the conduction band of ZnCdS nanorods to the valence band due to the lower band gap energy. As the conduction potential of ZnCdS is more negative than that of ZnS, the excited electrons will transit from the conduction band of ZnCdS nanorods to that of ZnS nanosheets, resulting in the separation of electron–hole pair. Due to the existence of internal fields, the potential barrier at the interface of the heterostructure prevents photogenerated back to ZnCdS nanorods, the photogenerated electrons have a longer lifetime. At the same time, sample #3 has higher electron carriers, meaning that the electrons could be rapidly transmitted to start reduction reaction with H2O, producing hydrogen, while the hole sacrificial agent L-lactic acid in the system consumed electrons, forming pyruvic acid and hydrogen (h+ + L-lactic → CH3COCOOH + H2). These phenomena effectively promoted the photoinduced electron–hole separation and resulted in the excellent photocatalytic performance. The better photocatalytic H2 reproduction of sample #3 than sample #2 can be ascribed to the lower charge transfer resistance and the stronger optical absorption, the lower charge transfer resistance will accelerate electrons' transition to participate the reduction reaction with H2O; and the stronger visible light absorption of sample #3 can provide more photogenerated electrons for hydrogen production (2H+ + 2e− → H2).
Fig. 8 The schematic illustration for electron charge transfer and H2 evolution mechanism for the Zn0.2Cd0.8S/ZnS nanocomposites. |
This journal is © The Royal Society of Chemistry 2021 |