Jia
Luo
,
Huaiyu
Li
,
Guo
Yu
,
Wenyuan
Xu
,
Hong
Yin
* and
Zhaohui
Hou
*
Key Laboratory of Hunan Province for Advanced Carbon-based Functional Materials, Hunan Institute of Science and Technology, Yueyang 414006, China. E-mail: 2017507027@hust.edu.cn; zhaohuihou@126.com
First published on 15th March 2022
Tin monosulfide (SnS) anodes have attracted much attention for lithium-ion batteries (LIBs) due to their excellent chemical stability, high theoretical specific capacity and outstanding reversibility. However, the slow kinetics and large volume expansion of intrinsic SnS electrodes in the conversion reaction process restrict their application to a certain extent. To address the poor conductivity and volume fluctuation, N-doped double-carbon-layer protective hierarchical structures decorating SnS nanotubes (N-DCSNs) are introduced by in situ polymerization directed using a g-C3N4 soft template. Particularly, N-doped double carbon layers provide fast transport channels for electrons and ions, affording decent conductivity and rapid ionic diffusion rate. Most importantly, the volume expansion of SnS during the charge–discharge cycles can be buffered owing to the confinement effect of the double carbon layer. Synergistic effects of N-DCSNs enhance the mechanical integrity and electrochemical kinetics during the charge–discharge process, leading to high-capacity retention and long-term stability properties. As a remarkable anode for LIBs, the N-DCSN electrode delivers high capacities of 911.5 and 511.3 mA h g−1 at 0.2 and 1.0 A g−1 after 270 and 1000 cycles, respectively. The feasible and versatile structure design can offer new ideas for the preparation and regulation of other transition metal sulfide anode materials, and provide a relevant experimental basis for the further development of lithium/sodium storage equipment.
Among various anode materials, metal chalcogenides based on conversion/alloying reactions are attractive because of their high theoretical specific capacity, outstanding chemical stability and eminent reversibility. In particular, as the voltage lag of metal sulfide is smaller than that of metal oxide, which makes the metal sulfide show higher energy efficiency for LIBs.7 A promising basal material for storing various alkali metal ions through the conversion/alloying reaction is tin monosulfide (SnS) with a unique two-dimensional layered structure.8 The layered structure provides abundant reaction sites for charge storage, which is conducive to e−/Li+ transport and electrolyte diffusion. The effect can improve the ion intercalation efficiency, which shows high theoretical specific capacity (782 mA h g−1), and has broad electrochemical application prospects in power storage devices.9 However, the complex lithium storage mechanism of SnS is based on the conversion reaction to form Li2S and Sn. The alloying reaction occurs at the same time to form a LixSnS alloy leading to some serious problems.10 First, a redox reaction will occur in the process of lithiation/delithiation to form multiphase structures, which will lead to slow kinetic problems. Second, the inherent electronic conductivity of SnS is poor, which will directly affect the rate performance of LIBs. Third, irrespective of whether a conversion reaction or an alloying reaction occurs, SnS will produce large volume strain in the electrochemical process, including electrode particle pulverization, deterioration or agglomeration, resulting in poor cycle performance.11
Relevant approaches are adopted to address these problems, such as combining with carbon materials,12–15 preparing nano hollow structures,7 doping and modification of heteroatoms.16–18 Carbon materials can play an important role in buffering volume change, enhancing ion and electron transport and reducing the size of anode materials by constructing a reasonable structure.19 Hollow nanostructures can not only inhibit metal agglomeration, but also expose more active sites to ensure the full use of electroactive materials. Additionally, nitrogen doping can also increase the electrochemical reactivity, conductivity and surface wettability of carbon, which is conducive to the diffusion of Li-ion through the interface between the carbon electrode and electrolyte.20 Jin et al. prepared N-doped carbon-coated SnS nanoparticles, which delivered a capacity of 741.4 mA h g−1 at 100 mA g−1 current density after 200 cycles, showing better cycling stability.7 Xia et al. prepared a SnS/C nanofiber membrane by a simple and general electrospinning method, which is directly used as an independent anode in LIBs, providing excellent electrochemical performance.16 However, few Sn-based anode materials have achieved a super-long cycle life of more than 500 cycles, which may be due to the fact that carbon has not been excavated well. In order to solve this problem, carbon matrix composite electrodes can be designed rationally by selecting a suitable carbon source. Due to the particularity of g-C3N4, it has been widely used in photocatalysis, electrocatalysis, supercapacitors and energy storage systems.21,22 The graphite phase C3N4 (g-C3N4) has a similar structure to graphene. It has a high specific surface area, easy synthesis, excellent chemical stability, environmental friendliness and high theoretical lithium storage capacity (524 mA h g−1).23 The g-C3N4 has been broadly applied for building soft templates or affording high-speed electronic channels to improve the Li-storage of metal sulfide. Yin et al. constructed nanoflower SnS2 based on g-C3N4 nanosheet composite materials as efficient anode electrodes of LIBs.24 It is worth noting that polyaniline (PANI) has the characteristics of high specific capacity, admirable redox reversibility, high conductivity, simple synthesis method, and low cost.25 It is widely used in chemical power supply and can alleviate the problem of poor cycling stability of LIBs. Therefore, the reasonable design of the carbon composite material can obtain excellent performance of anode electrodes.
In this study, N-doped double-carbon-layer protective hierarchical structures decorating SnS nanotubes (N-DCSNs) are introduced for addressing the poor conductivity and volume fluctuation by hydrothermal and in situ polymerization. Based on the structure design, the N-doped double-carbon layer provides abundant active sites and defects that help shorten ion and electron transport paths. In addition, it helps to maintain the mechanical integrity of the structure and stabilize SEI formation to buffer volume changes of SnS. Structural advantages enhance mechanical integrity and electrochemical kinetics during the charge–discharge process, leading to long-term stable lithium storage performances. The N-DCSN electrodes deliver high capacities of 511.3 mA h g−1 after 1000 cycles at 1.0 A g−1, and the coulombic efficiency can reach 95.9% after the first discharge cycle. This method can be extended to the preparation of other carbon-coated electrodes, aiming at improving the conductivity and structural stability of anode materials for LIBs.
(1) Preparation of bare SnS: Firstly, 0.5 g PVP was dispersed in 60 ml absolute ethanol by ultrasound, then 0.45 g SnCl2·2H2O and 0.15 g TAA were added successively, and were stirred for 30 min. Then the mixed solution was placed in a hydrothermal kettle and reacted at 180 °C for 12 h to obtain pure SnS nano flower balls.
(2) Preparation of CN/SnS composites: Firstly, melamine was placed in a crucible and heated to 550 °C at 5 °C min in the air of a muffle furnace for 4 h. When the temperature was reduced to room temperature, it was ground into powder to obtain g-C3N4. 0.5 g PVP and 2 g g-C3N4 powder were dispersed in 60 ml absolute ethanol by ultrasound. Then 0.45 g SnCl2·2H2O and 0.15 g TAA were added successively and stirred for 4 h. Then, the dispersion was placed in a hydrothermal kettle and reacted at 180 °C for 12 h. Finally, it was centrifuged, washed with ethanol several times and dried to obtain CN/SnS composites.
(3) Preparation of N-DCSNs: The CN/SnS composites prepared above were ultrasonically dispersed in 50 ml deionized water, and 0.3 ml concentrated HCl was added for ultrasonic uniformity. 0.45 g aniline monomer was added in an ice bath and stirred for several minutes, then 1.23 g ammonium persulfate was added slowly and was stirred for 12 h. After that, it was centrifuged, washed with deionized water several times, and dried in a 70 °C vacuum oven overnight. Finally, in a tubular furnace, the temperature was raised to 800 °C at a rate of 5 °C min−1 in Ar/H2 gas, the temperature was maintained for 2 h, and then cooled to room temperature to obtain N-DCSNs.
(2) Assembly of button batteries: The working electrodes were placed in the glove box protected by high-purity argon. The electrodes, diaphragms and lithium sheets were placed at the bottom shell of CR 2025 button batteries successively, an appropriate amount of electrolyte (1.0 M LiPF6 in EC: DMC: EMC = 1:1: 1 Vol% with 5.0% FEC) was injected. And the electrodes were packaged into coin half batteries for the electrochemical test.
(3) Electrochemical performance test: The CT2001A battery test system was used to test the cycle performance and rate performance of the batteries; the voltage range of the battery test was set to 0.01-3 V at 0.2 and 1.0 A g−1, respectively. The electrochemical workstation (Interface 1010E) was used to test the cyclic voltammetry and AC impedance of the batteries. The sweep rate range of cyclic voltammetry was 0.2–1.0 mV s−1.
Fig. 2 (a) XRD patterns of bare SnS, CN/SnS composites and N-DCSNs. (b) Raman spectrums of N-DCSNs. (c–f) XPS spectra of N-DCSNs for (c) Sn 3d, (d) S 2p, (e) N 1s, and (f) C 1s. |
In order to determine the carbon content and elemental composition of N-DCSNs, thermogravimetric analysis and XPS measurement are carried out. The TGA curve is shown in Fig. S2 (ESI†). The main weight loss temperature range is 400–600 °C, which can be attributed to the conversion from SnS to SnO2 and the gasification of carbon materials.28 Since the relative molecular weights of SnS and SnO2 are equal, the carbon content in the composite can be determined to be about 64.68%.15,29 In particular, the carbon materials could contribute some capacities as the active material.30Fig. 2c–f exhibit the XPS measurement spectra of Sn, S, N and C of N-DCSNs, and the full spectrum is shown in the ESI† (Fig. S3). Fig. 2c manifests that the high-resolution Sn 3d spectrum can be deconvoluted into two main peaks. The two peaks at 494.5 and 486 eV can correspond to Sn 3d3/2 and Sn 3d5/2 of Sn2+ in SnS, respectively.31 The S 2p spectrum can be divided into four main peaks (Fig. 2d), and the peak at 161.6 eV can be attributed to S 2p3/2 of SnS.32 Two peaks at 162.8 and 165.25 eV conform to the C–S–C heterocyclic configuration,33 and the weak peak at 167.1 eV is usually attributed to sulfate groups (C-SOx-C).34 These C-S-C bonds are rich in electron pairs, which is highly beneficial for improving the electrochemical reaction kinetics of SnS.16 The high-resolution N 1s spectrum in Fig. 2e shows that there are three peaks at 398.3, 400.1 and 400.6 eV, representing the pyridinic N, pyrrolic N and graphitic N, respectively.35 As shown in Fig. 2f, the main peak of the C 1s spectrum at 284.3 eV is attributed to the C–C/CC bond, while the small peaks at 286 and 286.6 eV are attributed to the C-N bond and C–O bond, respectively.36 The results indicate that nitrogen atoms are successfully doped at the edge or defect position of the carbonized PANI lattice. N-doped carbon can improve the reactivity and electronic conductivity by producing extrinsic defects.37 Initially, nitrogen doped carbon matrix can effectively reduce the energy barrier of lithiation and promote the rapid diffusion of Li+ and e− on the surface and inside of N-DCSN composites. Moreover, the introduction of pyridinic nitrogen and pyrrolic nitrogen can produce a large number of pores and surface defects on the carbon matrix, expose more active sites, and provide a shorter diffusion path for Li+ insertion.38 Therefore, N-doped carbon matrix coated SnS particles can enhance the lithium storage capacity and improve the electrochemical performance of LIBs.
In order to further explore the structure and morphology of N-DCSNs, the morphological characteristics of bare SnS, CN/SnS composites and N-DCSNs are characterized by SEM. The result of N-DCSNs is shown in Fig. 3a while the morphology of bare SnS and CN/SnS composites is displayed in the ESI† (Fig. S4). According to SEM, the N-DCSN composite presents the morphology of sandwich double carbon layer coated SnS nanotubes. The amount of exposed tubular structure of N-DCSNs is less than that of CN/SnS composites, which may be due to the partial tubular morphology covered by the PANI carbonization layer. However, the addition of the second carbon layer of PANI can well alleviate the volume expansion of SnS in the lithiation/delithiation process. Moreover, the PANI carbonization skeleton helps maintain the mechanical integrity of the structure, enrich the charge transfer channels, provide more lithium storage active sites, shorten the transmission path of ions and electrons, and accelerate the diffusion rate of Li-ions.25 By observing the TEM diagram of N-DCSNs (Fig. 3b), the double-layer carbon structure can be clearly seen in the sample, which matches the SEM image (Fig. 3a). The high resolution TEM (HRTEM) image (Fig. 3c) reveals clear lattice fringes with spaces of 0.293 nm and 0.342 nm, corresponding to the (101) and (120) planes of orthorhombic SnS, respectively.16 The selected area electron diffraction (SAED) pattern shown in Fig. 3d further confirms the existence of SnS, and different diffraction rings can be well matched to the (312), (211) and (120) planes of orthogonal SnS (JCPDS No. 39-0354).38 The EDX elemental maps (Fig. 3e–g) illustrate that C, N, Sn and S elements are evenly distributed in the composite.
Cyclic performance is an important factor for measuring the electrochemical performance of materials. The cycling properties of bare SnS, CN/SnS composites and N-DCSNs as anode materials for LIBs are tested at a current density of 0.2 A g−1 (Fig. 4d). The initial discharge specific capacity of the N-DCSN electrode can reach 1394.8 mA h g−1. Due to the formation of a SEI film, irreversible capacity is inevitably generated.43 In the subsequent cycle, the N-DCSN electrode decays slightly. At 44 cycles, the specific discharge capacity decreased to 727.6 mA h g−1. However, in the overall charge–discharge process, the coulombic efficiency is maintained above 100%. The high coulombic efficiency can be attributed to the high conductivity of the PANI carbonized layer and the structural defects produced by the g-C3N4 soft template, which synergetically accelerates the electron and ion diffusion rates. Interestingly, with the increase of the number of cycles, the discharge specific capacity even shows an upward trend. The as-prepared electrode can deliver a specific discharge capacity of 911.5 mA h g−1 at 0.2 A g−1 after 270 cycles. The increase of the specific discharge capacity may be attributed to the fact that the electrochemical grinding effect reduces the particle size of SnS nanoparticles in the continuous reaction. And the ultra-fine nanoparticles can effectively slow down the volume expansion, resulting in a higher reversible lithium storage capacity. In addition, the electrolyte will form a gel-like layer in the reaction process, which is also conducive to the increase of specific capacity.44 Compared with the N-DCSN electrode, the initial discharge specific capacity of the bare SnS electrode also reached 1084.7 mA h g−1 at 0.2 A g−1. However, due to the large volume effect in the process of charge and discharge, the attenuation range of the discharge specific capacity becomes larger with the increase of the number of cycles. The initial specific capacity of the CN/SnS electrode is only 779.4 mA h g−1, and the overall attenuation of specific capacity during charge and discharge is not as large as that of the bare SnS electrode, but it is still less stable than that of the N-DCSN electrode.
The long cycling stability of the N-DCSNs electrode is further reflected in Fig. 4e. The N-DCSN electrode also showed capacity attenuation after the first cycle at a high current density of 1.0 A g−1. However, with the increase in the number of subsequent cycles, the specific discharge capacity also tends to become stable. The discharge specific capacity of the N-DCSN electrode is still 511.3 mA h g−1 after 1000 cycles, which proves that the N-DCSN electrode has excellent cycling stability and capacity retention. The excellent electrochemical properties of N-DCSN electrodes can be ascribed to the structural advantages of the materials. SnS nanoparticles were evenly embedded into the g-C3N4 soft template. The g-C3N4 is cracked at high temperatures to produce a porous structure and increase the specific surface area of the material. The special structure helps shorten the Li+ and e− transport paths, and provides abundant active sites. N-doped carbon matrix has high conductivity, which speeds up the reaction kinetic rate of N-DCSN electrodes. Generally, if nanoparticles are exposed to electrolytes in a large area, too many side reactions will occur, resulting in the reduction of coulombic efficiency. Besides, the carbon layer is relatively fragile, and composites with a single carbon layer are more likely to collapse during deep cycling, resulting in a rapid capacity loss.45 Therefore, the double carbon layer can not only block the direct contact between SnS particles and electrolyte, but also inhibits the volume expansion of SnS particles in the lithiation/delithiation process. The dual functions of packaging tin based sulfide volume change and stabilizing the SEI layer are realized by using double carbon layers in the cycle,46 so that the coulomb efficiency, cycling stability and magnification performance of the N-DCSN electrode are greatly improved.
Electrochemical impedance spectroscopy (EIS) measurement can further explore the reaction mechanism of N-DCSN electrodes. Fig. 5a–b show the Nyquist diagram of bare SnS, CN/SnS and N-DCSN electrodes before the first charge/discharge and after 50 cycles at 0.2 A g−1 current density. In addition, the equivalent circuit model is also shown in Fig. S10, ESI.† The semicircle in the high frequency region of the Nyquist diagram is attributed to the surface film resistance (Rf) and the interfacial charge transfer resistance (Rct), while the slant in the low frequency region is attributed to the diffusion of Li+ in the active material.47 In the high frequency region of Fig. 5a, the semicircle diameter of the N-DCSN electrode is smaller than that of the bare SnS and CN/SnS electrode, indicating that the conductivity of the N-DCSN electrode is the largest among the three. The conclusion can also be drawn by comparing the Rct parameters of the N-DCSN electrode (24.24 Ω), CN/SnS electrode (57.19 Ω) and bare SnS electrode (61.77 Ω). Moreover, Fig. 5b reveals that the semicircle diameter of the N-DCSN electrode decreases significantly after 50 cycles, indicating that its conductivity increases further, which will help to enhance the stability of the interface between the electrode and electrolyte.48Fig. 5d and e show the Zre and ω−1/2 linear relationship of three electrode samples in the low frequency region, and it is fitted to Warburg factor σw. According to the Warburg factor (σw), the diffusion coefficient of the Li-ion (D value) can be directly determined, and the D value is negatively correlated with σw. The calculation formulas are as follows:49
D = R2T2/2A2n4F4C2σ2 | (1) |
ZRe = Re + Rct + σω−1/2 | (2) |
The relevant interpretation of the calculation formula is shown in the supporting literature (Depiction 1). The σw value of bare SnS before cycling (Fig. 5d) is the smallest, which can be attributed to the formation of a SEI film during the initial charge/discharge process of N-DCSN electrodes. Meanwhile, the comparison of discharge specific capacity in the first few cycles of the long-term cycling performance diagram (Fig. 4d) can also confirm this fact. Fig. 5e illustrates that the σw value of the N-DCSN electrodes changes slightly after 50 cycles. However, the σw values of bare SnS and CN/SnS electrodes increase significantly, indicating that the structure of electrodes collapses due to large volume strain. This fact can be attributed to the PANI carbon layer cutting off the direct contact between the electrode and the electrolyte, preventing side reactions and restraining electrolyte decomposition.47 It also shows that the limiting effect of the double carbon layer packaging structure prevents the electrode structure from being greatly affected after a long-term charge/discharge process, and still maintains a considerable Li-ion diffusion coefficient. The SEM images of the N-DCSN electrodes after rate performance and long-term cycles at 0.2 A g−1 proved this conjecture, as displayed in the ESI† (Fig. S11). The SEM image after 60 cycles showed that the morphology of N-DCSN electrodes did not change significantly. Even after 270 cycles, the structure remains remarkably intact, which is due to the synergistic protective effect of the double carbon layer. It is further confirmed that the excellent rate performance and long-term stability of N-DCSN electrodes are related to the special structure of the materials.
Galvanostatic intermittent titration (GITT) is a commonly used method to study the diffusion mechanism of solid ions, which is also used to measure the diffusion rate of Li+ in electrode films. The electrodes of the three materials were fully discharged at a current density of 200 mA g−1, then partially discharged at a current density of 100 mA g−1, and then open circuit relaxation was observed for 10 minutes for GITT measurement. The GITT curves of bare SnS, CN/SnS and N-DCSN electrodes are shown in Fig. 5c. The chemical diffusion coefficients of the three materials in LIBs are determined by formulas 3 and 4 (Depiction S2):
(3) |
(4) |
Fig. 5f illustrates the Li+ diffusion coefficient of the bare SnS, CN/SnS and N-DCSN electrodes during lithium intercalation. From 0.01 V to about 0.54 V, the GITT curve is downward, and the diffusion coefficient decreases. This can be attributed to the formation of a solid electrolyte interface (SEI) film at the electrode, which limits the diffusion of Li-ion. Then, due to the multi-step dealloying reaction, the diffusion rate is accelerated, corresponding to 0.68 V. Due to the conversion reaction of SnS (SnS + 2Li+ + 2e− → Sn + Li2S), the consumption of Li-ion is large, diffusion slows down, and the diffusion coefficient is the lowest at about 1.11 V. Finally, the diffusion rate is accelerated due to reversible transformation. The model shown in Fig. 6 illustrates the lithiation process, which is in accordance with the CV curve (Fig. 4a). During the lithiation process, Li+ will insert into SnS interlayers, causing crystal structure expansion. The hexagonal SnS will be transformed into face-centered tetragonal 2β-Sn and cubic Li2S by conversion reaction. After that, the orthogonal LixSn nanocrystals are formed by the alloying reaction. Furthermore, Li+ and SnS can be reconverted by dealloying and conversion reaction during the process of delithiation. In the whole process, the Li-intercalation barrier is reduced by the N-doped carbon matrix, making the lithiation/delithiation process reversible. In addition, strain of the crystal structure can be effectively relieved by the protection mechanism of the double carbon layer. Comparing the calculation results of the three materials, it can be seen that the average DLi value range of bare SnS and CN/SnS electrodes is about 10-7 cm2 s−1 in the voltage range of 2.1–0.01 V. The DLi value of N-DCSN electrodes increases from 10-7 to 10-6 cm2 s−1, showing the highest Li+ diffusion coefficient. The result reasonably confirms that the special N-doped double carbon layer structure of N-DCSN electrodes can successfully improve the wettability of the organic electrolyte on carbon materials, and provide a two-way ion/electron transport channel between the inner and outer layers.20 As a result, it becomes conducive to the diffusion of Li-ion through the interface between the carbon electrode and electrolyte, speeding up the diffusion rate.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d2ma00017b |
This journal is © The Royal Society of Chemistry 2022 |