Alexey A.
Noyan
ab and
Kirill S.
Napolskii
*bc
aMoscow Institute of Physics and Technology, 141700, Dolgoprudny, Russian Federation
bDepartment of Chemistry, Lomonosov Moscow State University, 119991, Moscow, Russian Federation
cDepartment of Materials Science, Lomonosov Moscow State University, 119991, Moscow, Russian Federation. E-mail: kirill@inorg.chem.msu.ru
First published on 15th March 2022
Porous anodic aluminum oxide (AAO) is a unique platform for many high-tech applications in nanotechnology, nanophotonics, and membrane science. Although scanning electron microscopy is the technique most widely used to measure the pore diameters of an AAO structure, this method accesses only a limited area of the structure and provides data with limited statistics. The AAO characteristics, averaged over the entire thickness of a porous film, can be measured by optical spectroscopy. In this paper, we demonstrate that the angular dependence of the transmittance of AAO porous films has several features caused by birefringence, which is used to measure the porosity of AAO membranes. This method of measuring porosity is accurate, precise, cheap, and does not require specific sample preparation procedures.
Fig. 1 shows a schematic of the AAO structure. The pore diameter of an AAO is much less than the wavelength of visible light, and thus, this kind of structure may be described in terms of the effective medium model. It is worth noting that AAO has a preferential direction along the pores. All directions in the plane of the AAO film are identical, whereas the direction along the pores, which is perpendicular to the AAO plane, is distinct. The presence of this extraordinary axis may result in a birefringence effect. Birefringence has been previously observed in various nanostructures with structural anisotropy, for example, porous GaN distributed Bragg reflectors,15 porous silicon,16 packed films of colloidal particles,17 and self-assembled sheets of carbon nanotubes.18 However, birefringence in AAO is poorly studied19,20 and is usually not considered.
The extraordinary (nex) and ordinary (nor) refractive indices of AAO can be determined as follows:19,20
nex2 = (1 − p)nAAO2 + pnair2, | (1) |
(2) |
It is worth noting that the model considers AAO cell walls as a homogeneous material neglecting inner and outer layers.21 This simplification is possible due to the low difference between the refractive indices of inner and outer layers.
For the AAO obtained in 0.3 M oxalic acid electrolyte at 5 °C and an anodization voltage of 44 V, the refractive indices, measured in reflection mode by the prism coupling technique for different polarizations of an incident beam, varied by 1.5–6%.22 It has been experimentally proven that the birefringence effect correlates with AAO porosity. However, no quantitative theoretical explanation has been provided.
In transmission mode, the birefringence in AAO has recently been observed.23 Although the theoretical explanation had been proven to fit the experimental data recorded at various incidence angles, the data obtained had not been applied to the calculation of some parameters of the AAO structure (such as porosity).
Scanning electron microscopy (SEM) is usually used to measure the pore diameter, interpore distance, and porosity of AAO. Although SEM can be used to easily and quickly obtain plane view and cross-sectional images, this method can access the structure only within a limited area and provides data with limited statistics. Moreover, parameters that are measured from the AAO surface do not correspond to the parameters of an average structure for the following reasons: (i) the top surface of AAO, formed at the beginning of anodization, is not identical to the structure formed later during steady-state anodization; (ii) in the cross-section, the cell walls do not crack along the diameter, and thus, only a lower-bound estimate of the pore diameter may be obtained; (iii) the bottom surface is covered with a barrier layer, which should be removed before measurements are made. To remove the barrier layer, chemical24 or ion etching25 procedures can be applied, however, both methods damage the AAO structure and may change the pore diameter. In some anodization regimes (e.g., hard anodization under diffusion control26 or cyclic anodization at a periodically changing voltage27), the porosity and channel diameter vary along the axis normal to the film. In this case, the SEM of the surface does not describe the whole structure, and measuring the average porosity may provide additional useful information.
The birefringence method to measure porosity that we present in this paper is based on transmittance measurements and therefore gives the average porosity of the sample, which is difficult to obtain with other techniques.
The residual Al was dissolved in a solution of Br2 in CH3OH (1:10 vol.) at room temperature. For some of the AAO films, the barrier oxide layer was removed by chemical etching in 3 M H3PO4 solution at room temperature with the electrochemical detection of the pore opening moment.33 The etching time following the pore opening moment was equal to 10 min.
To check the performance of the birefringence method in measuring porosity, a series of AAO films with various pore diameters were prepared. For this purpose, an as-prepared AAO porous film was etched in 2 M H2SO4 solution at 20 °C. The etching was performed in nine stages for about 20 min each. After each etching stage, the porous film was repeatedly washed in deionized water and dried before optical properties were measured.
The transmittance spectra of the AAO porous films were recorded using a PerkinElmer Lambda 35 spectrophotometer. The spectra were collected at the normal incidence of light on the AAO film surface from 200 to 1100 nm with a slit width of 1 nm. A spot size at the sample position of 2 × 2 mm2 was used.
The experimental setup for birefringence measurements is shown in Fig. 2. The photodiode measures the intensity of a laser beam with the wavelength λ = 659 ± 1 nm. The AAO film was placed between two crossed or parallel polarizers and rotated around an axis perpendicular to the optical axis. The planes of polarization of the polarizers form a 45° angle with the rotation axis. The photodiode was connected to the ammeter that measured the short circuit photocurrent. The short circuit photocurrent of the Vishay BPW21R photodiode is linear over illumination; hence the current was recorded as the laser beam intensity in arbitrary units.
Δn = nex − nor. | (3) |
A schematic illustration of the laser beam path through a porous AAO film is shown in Fig. 3. The mean refraction angle (β), according to Snell's law, is:
(4) |
Fig. 3 Birefringence in AAO. TE and TM modes of light transmit with different effective refractive indices. |
In the case of birefringence, an incident beam is divided into two rays: the transverse electric (TE) mode (ray #1) with an electric field perpendicular to the plane of incidence and the transverse magnetic (TM) mode (ray #2) with an electric field in the plane of incidence. TE and TM modes of light transmit with different, but close refractive indices n1 and n2, respectively, and at different, but close, angles, β1 and β2.
n1 = nor | (5) |
(6) |
As shown in Appendix 1 in the ESI,† (5) and (6) yields:
n2 − n1 = sin2βΔn | (7) |
The optical path difference (δ) between rays #1 and #2 determines the intensity after interference. The equation for δ is derived in Appendix 2 in the ESI:†
(8) |
From (7) and (8), one can derive:
(9) |
(10) |
(11) |
(12) |
In the case of parallel polarizers:
(13) |
Instead of the transmittance of the membrane, the reflectance may be measured. In this case, the optical path difference δr will be twice δ derived for transmittance in eqn (9).
In raw data, the envelope of the maxima of both the I⊥(θ) and I‖(θ) curves decreases with θ. This behavior is caused by an increase in the reflectance of the AAO film with the rotation angle. To compensate for this effect, the intensity (I⊥ or I‖), measured after the polarizer 2 (Fig. 2), was normalized to the intensity of the laser beam passed through the polarizer 1 and the sample (Ip1(θ)). In the absence of the second polarizer, no interference of polarized waves occurs, and Ip1(θ) is monotonous without maxima or minima.
Specific points (extrema or the points of intersection) corresponding to δ/λ of 0.25, 0.5, and 0.75 are indicated in Fig. 4 by circles, triangles, and squares, respectively. The θ positions of these points were used to calculate β using (4), taking into account the effective refractive index (n) of the films (Appendix 3 in the ESI†). Then, the birefringence, Δn/n, was found according to (9), using the thickness of the AAO film, h = 52.5 ± 0.5 μm, determined from the cross-sectional SEM images. The results are listed in Table 1.
δ/λ | θ, ° | β, ° | Δn/n | p, % | |
---|---|---|---|---|---|
As-prepared AAO film | 0.25 | 35.1 | 20.9 | 0.0147 | 10.1 |
0.5 | 50.8 | 28.7 | 0.0152 | 10.4 | |
AAO film after barrier layer etching | 0.25 | 28.3 | 17.5 | 0.0210 | 14.7 |
0.5 | 41.6 | 24.9 | 0.0204 | 14.2 | |
0.75 | 53.1 | 30.5 | 0.0200 | 14.0 |
The values of Δn/n obtained were used to refine nAAO and calculate the porosity (p) by an iteration algorithm described below. The dependence of Δn/n = 2(nex − nox)/(nex + nox) on the porosity of the AAO film is shown in Fig. 5. The ordinary and extraordinary refractive indices were calculated by (1) and (2), using nair = 1.00. As the starting point, the refractive index of the AAO cell walls, nAAO, was taken as equal to 1.765 (the refractive index of corundum at 660 nm34). The following iteration algorithm was used (i is the iteration step number):
Fig. 5 Dependence of the birefringence on the porosity of the AAO film. Data calculated for two values of nAAO are shown: 1.765 (dashed line) and 1.67 (solid line). |
1. The dependence of Δn/n on the porosity (p) was calculated using nAAOi.
2. The porosity pi+1 was determined from the graph.
3. nAAOi+1 was calculated by substituting pi+1 into (2)
4. Steps #1–3 were repeated until the changes in nAAO and p became lower than 1%.
After three iterations, the refined value nAAO = 1.67 was obtained. This value is in good agreement with the refractive indices of amorphous Al2O3 films formed using different methods: reactive sputtering (nAl2O3 = 1.6335), electron beam evaporation (nAl2O3 = 1.60–1.7136), and spray pyrolysis (nAl2O3 = 1.5836). The close value of the refractive index of the AAO cell walls (nAAO = 1.64) was obtained for porous films formed in selenic acid electrolyte.37 A substantially lower value nAAO = 1.55 was found for the AAO film prepared in 0.3 M oxalic acid electrolyte at 40 V.38 However, in this case, the geometrical parameters were measured with low accuracy based on SEM data. The calculated values of AAO porosity for the case of nAAO = 1.67 are listed in Table 1.
It is worth noting that knowledge of the intrinsic value of nAAO is not critically important in the birefringence method for measuring porosity described in this work. If nAAO differs from 1.67 by 2%, the error in Δn/n is 5.5%, which results in a relative error of 5.5% in the porosity. In comparison, if porosity is determined from eqn (1) with known n and nAAO, a 2% error in nAAO results in a relative error of 36% in the porosity.
The shifts of the curves in Fig. 4 for as-prepared and etched AAO films are well-defined, allowing the detection of the increase in porosity during the barrier layer etching with high precision. According to birefringence measurements, the porosity increased from 10.3% to 14.3%.
In order to show that the I⊥(θ) and I‖(θ) curves correspond to the functions (10) and (13) over a wide range of θ, the δ/λ ratio was calculated for each angle from the experimental data (Fig. 4). (10) and (13) as the backward equations for δ/λ have an infinite number of solutions. The correct solution was selected for each angle, taking into account that the function is monotonous, continuous, and . From these assumptions, a single solution for each angle exists. For instance, for the AAO film after barrier layer etching dependence can be given as the following piece-wise function:
at θ from −41.6° to 41.6° (41.6° angle corresponds to δ/λ = 0.5);
at θ from −60° to −41.6° and from 41.6° to 60°.
According to (9), should be linearized in coordinates with the slope . The experimentally observed dependence of δ/λ on is shown in Fig. 6 by scatters. As the data (Fig. 4) do not perfectly fit the 0–1 range, they were dragged as shown in Appendix 4 in the ESI,† to avoid function jumps. The experimental data presented in Fig. 6 fit perfectly to linear functions, which confirmed that the theory and the experiment were consistent. The values calculated from the slopes are listed in Table 2. The calculated porosity of both the as-prepared AAO film and the membrane after barrier layer etching agrees with the values in Table 1.
Measurement geometry | Slope | Δn/n | p,% | |
---|---|---|---|---|
As-prepared AAO film | Crossed polarizers | 1.81 | 0.0141 | 9.6 |
Parallel polarizers | 1.88 | 0.0146 | 10.0 | |
AAO film after barrier layer etching | Crossed polarizers | 2.63 | 0.0210 | 14.7 |
Parallel polarizers | 2.45 | 0.0195 | 13.6 |
Linearization of the dependence of δ/λ on does not improve the accuracy of the porosity calculation but has an advantage in determining the porosity of thin films when points corresponding to the specific values of δ/λ may not be observed. In particular, for a membrane with porosity of 10%, the intersection of angular dependencies of I⊥ and I‖ can be observed only for the samples thicker than 15 μm.
To check the performance of the birefringence method in measuring porosity over a wide range, a series of AAO films etched in 2 M H2SO4 solution at 20 °C for up to 3 hours was prepared. The experimental dependences of I⊥/Ip1 and I‖/Ip1 on the rotation angle of the AAO film are shown in Appendix 5 in the ESI.† The angular dependence was used for the calculation of the mean porosity of the films under study. Then, an average pore diameter (Dp) was calculated using the equation:
(14) |
Fig. 7 SEM image of the as-prepared AAO porous film (a) and the same film after etching in 2 M H2SO4 solution at 20 °C for 3 hours (b). The top surfaces of the films were measured. |
Fig. 8 Dependence of an average pore diameter on the etching duration in 2 M H2SO4 solution at 20 °C. |
According to SEM, the porosity of the as-prepared film is 10 ± 1% (Dp = 33.5 ± 1.6 nm), whereas the porosity of the etched for 3 h film is 18 ± 1% (Dp = 45.0 ± 1.2 nm). Hence, SEM data are in agreement with birefringence measurements (Fig. 8). However, these methods allow different film parameters to be obtained: the mean porosity of the whole membrane is measured with the birefringence method, and only the film surface is observed on SEM.
Specificity of the birefringence in AAO is that the difference between extraordinary and ordinary refractive indices, Δn, is small in relation to the mean effective refractive index, n. For the series of AAO films obtained in 0.3 M oxalic acid electrolyte at 40 V and electrolyte temperature of 0 °C, Δn/n varied from 0.014 to 0.028. The birefringence Δn/n increases with the rise of porosity.
The birefringence effect in AAO was applied to calculate the refractive index of the AAO cell walls and film porosity for the first time. Only the AAO film thickness and the effective refractive index, which can be obtained easily by SEM measurements and analysis of Fabry–Pérot oscillations, are needed to measure these parameters.
The high sensitivity of the birefringence effect to the AAO porosity was proved experimentally. Even after barrier layer dissolution with electrochemical detection of the pore opening moment, an increase in the AAO porosity was unambiguously detected. A constant etching rate was observed in a series of AAO porous films etched in 2 M H2SO4 solution at 20 °C.
It is worth noting that eqn (1) and (2) were derived without assumptions on the 2D hexagonal ordering of the pores, and, thus, the measurements are not affected by the domain boundaries and other defects of porous structure. High accuracy, precision, low cost, and an easy sample preparation procedure make the method developed in this work an effective tool to measure the porosity of AAO films. The absence of quantitative approaches to solve this task using other techniques will guarantee worldwide interest in the method from scientists working in various areas of nanotechnology, membrane science, and other fields that we cannot yet envision. The suggested approach can be applied to measure the porosity of other optically transparent materials, containing aligned cylindrical channels, such as anodic titanium oxide, porous silicon and silicon oxide, track-etched membranes, and porous films based on diblock copolymers. Another promising application of the birefringence method is mapping of AAO to study the spatial distribution of non-homogeneity and anisotropy of its structure. In this case, a laser beam spot size much smaller than the lateral size of Al grains or AAO domains should be provided.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d2ma00111j |
This journal is © The Royal Society of Chemistry 2022 |