Jaewook Shinab,
Hyeonmuk Kanga,
Yongju Leea,
Sang Hyeon Hac and
EunAe Cho
*ab
aDepartment of Materials Science and Engineering, Korea Advanced Institute of Science and Technology (KAIST), 291 Daehak-ro, Yuseong-gu, Daejeon, 34141, Republic of Korea. E-mail: eacho@kaist.ac.kr; Tel: +82-42-350-3317
bAdvanced Battery Center, KAIST Institute for NanoCentury, Korea Advanced Institute of Science and Technology (KAIST), 291 Daehak-ro, Yuseong-gu, Daejeon, 34141, Republic of Korea
cAgency for Defense Development, Yuseong P.O. Box 35-41, Daejeon, 34188, Republic of Korea
First published on 9th February 2022
The thermal battery, a key source for powering defensive power systems, employs Li alloy-based anodes. However, the alloying increases the reduction potential of Li which lowers the overall working voltage and energy output. To overcome these issues, Li alloy must be replaced with pure Li. Utilizing pure Li requires a structure that can hold liquefied Li because the working temperature for the thermal battery exceeds the melting point of Li. The liquefied Li can leak out of the anode, causing short-circuit. A Li–Fe electrode (LiFE) in which Fe powder holds liquefied Li has been developed. In LiFE, higher Li content can lead to higher energy output but increases the risk of Li leakage. Thus, Li content in the LiFE has been limited. Here, we demonstrate a novel core–shell electrode structure to achieve a higher energy output. The proposed core–shell LiFE incorporates a high Li content core and a low Li content shell; high energy comes from the core and the shell prevents the Li from leakage. The fabricated core–shell structured electrode demonstrates the high energy of 9074 W s, an increase by 1.66 times compared to the low Li content LiFE with the conventionally used Li content (5509 W s).
![]() | ||
Fig. 1 (a) A graphical representation of the thermal battery operation. (b) A graphical illustration of the LiFE before and after Li incorporation. |
For the thermal battery anode, Li can be considered as the active Li source material. However, due to the low melting point of Li (180.5 °C), Li liquefies during activation, causing short-circuit by Li leakage and migration to the cathode side. As an alternative, Li–Si alloy or another type of Li alloys are utilized owing to their reliable physical state at the elevated operation temperature.3 Li alloys utilized in the thermal batteries have a significantly higher melting point (Li–Si alloy Tm: 650–800 °C) that they remain solid-state during the thermal battery operation.3 However, as the consequence of altering the electronic structure of Li by alloying, the anode reduction potential increases. Higher potential from the anode results in lower overall cell potential, thus lower energy output.
To mitigate the compromised output from the anode and to prevent short-circuit by Li leakage, Li electrodes with iron particles such as liquid anode network (LAN, by Aerospatiale Batteries (ASB)) have been proposed as an alternative anode system. The Li–Fe electrode (LiFE), first proposed in Catalytic Research Laboratory, is composed of Fe powder in Li matrix. Fe powder holds liquid Li during thermal battery operation. This system fully utilizes the thermodynamic potential of the Li because the Fe does not alloy with Li and the reduction potential of Li is unchanged. Thus, the Li–Fe electrode can produce higher full cell voltages than the conventional Li–Si alloys, owing to the lower reduction potential as an anode. However, to avoid short-circuit and gain reliability, a sufficient amount of Fe powder should be included in the LiFE and the Li composition must be low (Fig. 1b).4–6 However, the low Li composition leads to low energy density. An innovative methodology must be incorporated to be able to utilize the LiFE system with high energy and power density.
In LiFE, the low Li composition anode has low energy but good reliability. The high Li composition anode has high energy but bad reliability. This work presents a core–shell type electrode design to combine the two types of Li composition. The newly proposed electrode brings out the benefits and mitigates the disadvantages from the low-Li and high-Li composition electrodes. We have implemented the high Li composition electrode as the core and low Li composition electrode as the shell. The core high-Li electrode may liquefy and become physically unstable, but the shell low-Li electrode will act as a barrier for liquid Li from escaping and causing short-circuit. In addition, owing to the high-Li core, the overall electrode has a high energy density. The core–shell LiFE is characterized by scanning electron microscopy (SEM), electrochemical discharge, and impedance electrochemical spectroscopy (EIS).
The core–shell LiFE was fabricated with the 13 wt% Li–Fe roll-pressed into 0.2 mm thickness slab and 20 wt% Li–Fe roll-pressed into 0.8 mm thickness slab. The 20 wt% Li–Fe slab was sandwiched in between the 13 wt% Li–Fe slabs. The sandwiched slabs were then roll pressed into 0.55 mm thickness as the core–shell LiFE.
To fabricate the prepared LiFEs into hollow-structured anodes of thermal battery, the rolled-out slabs (13 wt% LiFE, 20 wt% LiFE, and core–shell LiFE) were punched out using disks with 56 and 7.4 mm diameter, concentrically. The anode was then pressed with a Ni mesh sealed in a Ni cup. The Ni grid has diamond shape windows and 30 mesh count.
The electrochemical discharge was performed with applied pressure at an elevated temperature. The assembled full cell was first pressed with 80 Kg F pressure with two hot plates (top and bottom). Once the desired pressed has been reached, the temperature of the hot plates was raised to 500 °C. Then, the open-circuit voltage was measured for about 2 min and 8.89 A current was applied to the full cell until the voltage drops to ∼0 V.
The core–shell structured LiFE was designed to be composed of 20 wt% LiFE core and 13 wt% LiFE shell. Recently, Im et al. in 2018 demonstrated that 13 wt% Li is the maximum amount of Li content without causing Li leakage in LiFE.7 Thus, for the shell, 13 wt% Li LiFE is chosen to prevent Li leakage. For the core, to increase the energy density, 20 wt% Li LiFE has been employed. The optical images of the roll-pressed 13 wt% Li and 20 wt% Li slabs and step-by-step process of fabricating the core–shell LiFE are provided (Fig. 3). Fe powder was mixed with liquefied Li metal with 13 and 20 wt% Li. Then, the mixtures were poured into ingots, which were roll-pressed into slabs to obtain LiFE (Fig. 3a and b). Then, a 20 wt% LiFE was sandwiched with two slabs of 13 wt% LiFEs to form the core–shell structured electrode (Fig. 3c).
![]() | ||
Fig. 3 (a) Optical images of the 13 wt% Li and 20 wt% Li slabs. (b) The fabrication process of the core–shell LiFE. (c) Prepared core–shell LiFE. |
One of the key features of LiFE is the fact that the Li and Fe do not chemically react and hence the electronic structure of Li is unaltered. Unaltered Li state gives the lowest anode potential same as the pure Li and highest voltage output. To examine whether or not the Li and Fe chemically react to form other phases, PXRD patterns of Fe powder, 13 wt% Li LiFE, 20 wt% Li LiFE, and core–shell LiFE are obtained (Fig. 4a). All four samples show sharp peaks around 44.8° and 65.1° representing crystalline Fe phase and a broad peak around 18° representing the amorphous phase Kapton tape used to seal the samples to prevent from air contamination. The air can react with Fe and Li to form Fe2O3, Li2O, and Li3N.8–10 The uncontrolled amount of these unwanted side products add inactive mass and volume, leading to lowering gravimetric and volumetric energy density. Because the PXRD patterns are measured with Cu Kα radiation, the Li metal phase cannot be detected.11 No additional crystalline nor amorphous phase has been found. These results signify that even after mixing liquefied Li with Fe powder at an elevated temperature of 350 °C, Fe and Li did not react to form other phases and that the chemical state of Li has not been altered.
![]() | ||
Fig. 4 (a) XRD patterns for the three LiFE and the Fe powder. SEM images of the (b) 13 wt% Li LiFE and (c) 20 wt% Li LiFE. |
The SEM images of the 13 wt% Li LiFE and 20 wt% Li LiFE are obtained to better understand the electrode morphology (Fig. 4b and c). Both images show light contrasts in dark background. The light contrasts represent Fe particles coated with Li metal. The Li metal cannot be clearly imaged in the SEM because the Li atoms have very little interaction with e− in the SEM.12,13 The main difference between the 13 wt% Li LiFE and the 20 wt% Li LiFE is the spacing among the Fe particles. Because Li has a significantly lighter density (0.534 g cm−3) than Fe (7.874 g cm−3), in terms of volume, 13 wt% and 20 wt% Li composition correspond to 69 v% and 79 v%, respectively. Thus, the Fe volume is 31 v% and 21 v% in 13 wt% and 20 wt% LiFE, respectively. The spacing among the Fe particles in SEM represents the difference in the volumetric composition of Fe. The 13 wt% Li LiFE, compared to the 20 wt% Li LiFE has significantly more compacted Fe particle distribution. Such a compacted distribution likely has a better ability to hold liquefied Li in place and better electrical pathways through the connected Fe particles. Due to the less compacted Fe distribution, 20 wt% Li LiFE is more likely to have liquid Li leakage that leads to short-circuit and loss of active Li for electrochemical discharge.
Upon punching out the 0.55 mm thick LiFEs in hollow disks, the electrodes were weighed in a dry room (Table 1). All four electrodes have the same volume (1331 mm3). As expected, 13 wt% Li LiFE has the highest electrode mass, followed by core–shell LiFE and 20 wt% Li LiFE. Based on the mass of the electrodes, the overall Li content of the core–shell LiFE has been calculated to be 17.2 wt%. In thickness, the core–shell electrode is composed of 0.111 mm thick 13 wt% Li LIFE in the top and bottom layers and 0.328 mm thick 20 wt% Li LIFE core layer. Based on the electrode mass, the amounts of active Li available for the electrochemical discharge can be calculated; 13 wt% Li, 20 wt% Li, and core–shell LiFE have active Li mass of 0.37, 0.42, and 0.41 mg mm−3, respectively. Compared to the 13 wt% Li LiFE, by incorporating the core–shell LiFE, the electrode mass has decreased by 16% but the active Li mass has increased by 11%. As a result, the theoretical capacity of each LiFE is 6841, 7818, and 7679 A s for 13 wt% Li, 20 wt% Li, and core–shell LiFE, respectively. These capacities are calculated based on the specific theoretical capacity of Li: 13961 A s g−1.
13 wt% Li LiFE | 20 wt% Li LiFE | Core–shell LiFE | |
---|---|---|---|
Electrode thickness (mm) | 0.55 | 0.55 | 0.55 |
Electrode volume (mm3) | 1331 | 1331 | 1331 |
Electrode mass (g) | 3.77 | 2.78 | 3.18 |
Active Li mass (g) | 0.49 | 0.56 | 0.55 |
Specific Li mass (mg mm−3) | 0.37 | 0.42 | 0.41 |
Theo. Cap. (A sec) | 6841 | 7818 | 7679 |
The punched out LiFEs were assembled into thermal battery anodes (Fig. 5a). The LiFE is first stacked and pressed with Ni mesh to hinder Li leakage. The pressed LiFE is then placed in a Ni cup and the edge of the cup was bent inward so that the Li leak does not occur from the edges. When the full thermal battery cell is assembled, the cell components are pressed together to improve the packing density and electrical contact. The anode along with the electrolyte and cathode pellets are stacked together in between a set of Au coated stainless steel current collectors (Fig. 5b). The FeS2 is utilized as the cathode active material with 73.5 wt% composition and 26.5 wt% of electrolyte.14–17 To maximize the effect of LiFE anode and minimize any error from the cathode, an excess amount of cathode was utilized; 11.92 g of cathodes which contain 8.76 g FeS2 (45427 A s capacity) is used. Since theoretical capacity of Li and FeS2 is 13
961 and 5185 A s g−1, respectively, capacity of the cathode is roughly 6 times the capacity of anodes. The electrolyte contains LiF–LiCl–LiBr eutectic salt with MgO as a binder. The eutectic salt has a melting point (∼430 °C) lower than the thermal battery operation temperature, 500 °C. This salt is utilized to maximize the Li diffusion during the battery operation and for stable operation of the thermal battery. On the other hand, the MgO binder which does not melt during the battery operation was utilized to keep the structural integrity of the electrolyte during the battery operation. 2.48 g of electrolyte was utilized to ensure the structural integrity of the electrolyte pellet and minimize the Li+ ion diffusion pathway. After all the thermal battery components have been stacked together, the full cell was held together by heat resisting tape (Fig. 5c).
![]() | ||
Fig. 5 (a) Schematic illustration of the thermal battery anode preparation. (b) Schematic illustration of the thermal battery assembly. (c) An optical image of the assembled thermal battery. |
13 wt% Li, 20 wt% Li, and core–shell LiFE anodes have been assembled into full thermal battery cells and their discharge performance has been measured (Fig. 6). During the discharge test, the full cells undergo three different phases: solid-state, liquid-state, and discharge. In the beginning, the prepared cell is at the solid-state. To measure their discharge performance, the full cells are heated to 500 °C, so that the electrolyte will liquefy. Once the electrolyte has been melted, the cells are in the liquid-state and open-circuit voltage (OCV) can be measured. The OCV represents the Gibbs free energy difference between the cathode and the anode and can be considered as a characteristic parameter for judging the state of discharge.18 The OCV at the end of liquid state is 2.05 V, 1.97, and 2.06 V, for 13 wt% Li, 20 wt% Li, and core–shell LiFE, respectively (Fig. 6a, c and e). The core–shell LiFE has the highest OCV with 13 wt% LiFE close second. These two have a typical OCV for the LiFE anode and FeS2 based cathode.7 On the other hand, the OCV for the 20 wt% Li LiFE is significantly low compared to the other two. In addition, while the 13 wt% and core–shell LiFE electrodes have fairly stable OCV during the liquid-state, the 20 wt% LiFE electrode has a sudden drop in OCV around 20–30 s before the discharge phase. This sudden drop in the OCV is likely a result of a Li leakage that causes short-circuit. During the short-circuit, some portion of the Li and FeS2 reacts with each other and become inactive for electrochemical discharge.19 Such phenomenon is called self-discharge. Although the short-circuit only lasts for a few seconds, the OCV has gone down due to reaction between Li and FeS2.
The cells were kept in the liquid-state for roughly 2 min. After the 2 min, the constant current was applied to measure discharge performance. Immediately after the current was applied, the voltage dropped to an onset potential of 1.91 V, 1.89 V, and 1.92 V for 13 wt% Li, 20 wt% Li, and core–shell LiFE, respectively (Fig. 6a, c and e). The core–shell LiFE and 13 wt% Li LiFE have higher onset potential than the 20 wt% Li LiFE. This trend is consistent with the OCV's. The onset potential for the 20 wt% Li LiFE is lowest due to the Li leakage. The soft short circuit causes the Li react with cathode materials that increases the overpotential. The constant current was applied continuously until the voltage has reached 1.5 V. The time for the cells to reach the 1.5 V represents the useable capacity. The duration is 360, 258, and 560 s which corresponds 3204, 2296, and 4984 A s capacity, for 13 wt% Li, 20 wt% Li, and core–shell LiFE, respectively (Fig. 6a, c, e, and Table 2). The core–shell LiFE has the highest capacity and the 20 wt% Li LiFE has the lowest capacity due to Li leakage. The leaked Li reacted and inactivated a significant portion of Li anode and FeS2 cathode. The lack of available active materials leads to lower capacity. The 13 wt% Li LiFE's capacity is the baseline capacity where the Li leakage is prevented but has limited in capacity due to the lack of Li composition. On the other hand, the core–shell Li LiFE has 1.55 times the capacity as the 13 wt% Li LiFE. Such a substantial increase in capacity is coming from the high Li content core of the electrode. The core–shell LiFE not only has stable thermal battery operation but also has high capacity.
13% Li | 20% Li | Core–shell | |
---|---|---|---|
Time@1.5 V (sec) | 360 s | 258 s | 560 s |
Cap. (A sec) | 3204 | 2296 | 4984 |
Cap. Yield (%) | 47 | 29 | 65 |
To determine the state of thermal batteries after discharge, optical images of the discharged cells are provided in Fig. 6b, d and f. Compared to the pristine state of the thermal battery (Fig. 5c), color changes can be observed. Generally, all cells have the heat resistant tape turning dark due to carbonization and the gold coated stainless steel current collector changing to reddish-orange due to oxidation of stainless steel. These changes are present in all three cells and deemed little significance to the electrochemical discharge performance. The important change can be observed in the 20 wt% Li LIFE. Center of the cell has been filled with black material. The spots of the black material can be observed on the current collector as well. This black material is most likely a result of the Li leakage. During the liquid-state, Li from the 20 wt% Li LiFE leaked out and reacted with FeS2. On the other hand, the other two LiFEs do not show any sign of such Li leakage. The absence of leakage further supports the stability of 13 wt% Li and core–shell LiFEs.
Besides the electrochemical discharge performance and the observation of Li leakage, further characterizations are necessary to determine the electrode characteristics. The distribution of Fe has been observed under SEM. However, The Li distribution in LiFE is difficult to observe because Li atomic number is too low for the electron based microscopy techniques. To characterize Li morphology, electrochemical characterization techniques are proposed in this study (Fig. 7). First, expected Li morphologies are illustrated in Fig. 7a. During the mixing process between Li and Fe, liquefied Li mixes with Fe particles. When the Li solidifies, it forms a layer of Li coating on the Fe surface. In the low Li content electrode (13 wt% LiFE), the Li layer on the Fe surface will be thinner and more uniformly distributed. Due to such morphology, there will be more pores among the particles thus it has higher Li surface area. On the other hand, in the high Li content electrode (20 wt% LiFE), the Li layer on the Fe surface will be thicker and less uniformly distributed. Therefore, there will not be as many pores between the particles has lower Li surface area.
The surface area of Li was compared among the LiFEs by employing electrochemical techniques; electrochemical stripping and deposition technique and electrochemical impedance spectroscopy (EIS). For the electrochemical measurements, symmetric cells of the respective LiFEs with liquid organic electrolyte were assembled. Electrochemical stripping and deposition characteristics of Li in the organic electrolyte system is well known in the lithium-ion battery research.20 During the deposition, Li deposits as a dendritic form. Due to the low reduction potential of Li, the organic electrolyte decomposes on the surface of Li and deposits as thick solid-electrolyte interphase (SEI), which is known to be highly resistive and impedes Li+ ion diffusion.21,22 On the surface of the dendrites, the electrolyte decomposition product, SEI forms. Electrochemically stripping the Li causes the dendrite to be detached from the Li and the detached dendrite becomes electrochemically isolated due to the insulating SEI layer. These detached Li is called “dead Li”. Repeatedly depositing and stripping the Li generates more “dead Li”. When more “dead Li” is formed on the Li surface, it causes increased electrochemical polarization and impedance. Given the same current density of electrochemical reactions, lower Li surface area will form larger dendrite. Thus, the dendrite is more likely to detach during electrochemical stripping. Lower Li surface area will have more “dead Li” formation, thus higher polarization and impedance. The degree of “dead Li” formation is inversely proportional to the Li surface area.
The polarization can be measured by observing the overpotential applied during the electrochemical deposition and stripping. 100 repeated electrochemical deposition and stripping cycles were performed on the symmetric cells (Fig. 7b). The polarization during the beginning of the repeated cycles varies, because of activation. The Li surface may have some amount of oxide that need to be activated and the bare Li surface gets covered with the SEI. The most amount of electrolyte decomposition, or formation of SEI, occurs during this activation period. After about 20 cycles (40 h), the polarization starts to stabilize. After 100 cycles (200 h), the polarization is fully stabilized. Throughout the cycles, the 20 wt% Li LiFE has the highest polarization. To observe the polarization more closely, the last five cycles are zoomed-in (Fig. 7c). During the deposition reaction the voltage increases and during the stripping reaction the voltage decreases. The polarization can be presented by ΔV:
ΔV = Vstripping − Vdepositing | (1) |
In addition to the polarization, impedance can be measured to compare the Li surface area. Similarly, the impedance is also inversely correlated to the surface area.23 The EIS has been measured for the assembled symmetric cells after one electrodeposition and electrostripping reaction cycle. During the electrochemical cycle, the electrolyte molecules start to decompose and form an insulating SEI layer on the Li surface. The amount of SEI layer is inversely proportional to the Li surface area. Measuring the Li+ ion diffusion through the SEI layer allows for the comparison among the Li surface area. All three EIS spectra show a quasi-semicircle and Warburg impedance tail. The impedance at the end of the quasi-semicircle represents the Li+ ion diffusion through the SEI layer. The impedance is 104, 159, and 128 Ω for 13 wt% Li, 20 wt% Li, and core–shell LiFE, respectively (Fig. 7d). As expected, the 13 wt% Li LiFE has the lowest impedance and 20 wt% Li LiFE has the highest impedance. These indicate that the 20 wt% Li LiFE has smallest Li surface area and 13 wt% Li LiFE has largest Li surface area. The core–shell LiFE has a medium amount of impedance because it contains both the high and low Li surface area. The impedance measurements show a consistent trend as the polarization measurement. This further supports and surface area of the Li in the respective LiFEs. Since having more Li surface area is correlated to having more uniform Li distribution, having uniform Li distribution helps to produce stable thermal battery operation.
![]() | ||
Fig. 8 (a) Energy density profile of the three LiFE cells above 1.5 V. (b–d) Schematic illustration of the three LiFE cells in solid- and liquid-state. |
Based on the electrochemical discharge performance of the three thermal batteries, a schematic illustration of the LiFEs during thermal battery operation is provided (Fig. 8b and c). Before the thermal battery activation, all LiFEs are in solid-state. Upon activation, Li liquefies. When the Li liquefies, depending on the Li content, Li can remain in LiFE or leak out. In the 13 wt% low Li content, even when the Li is liquefied, the Li does not leak (Fig. 8b). However, it has limited energy density due to the low Li content threshold. On the other hand, in the 20 wt% high Li content, when the Li is liquefied, the Li leaks out and causes short-circuit (Fig. 8c). As a result, 20 wt% Li LiFE has even lower energy density than the 13 wt% Li LiFE. Lastly, to increase the energy density by increasing the Li content and to prevent Li leakage by decreasing the Li content, core–shell LiFE is fabricated. The core contains 20 wt% Li LiFE and the shell 13 wt% Li LiFE. The core may be unstable and Li may leak from the core, the Li does not leak out through the shell. By covering the 20 wt% Li with 13 wt% Li, the Li leak is prevented, even when the Li is liquefied (Fig. 8d).
This journal is © The Royal Society of Chemistry 2022 |