Jingjie Luo‡
,
Fengxiang Shan‡,
Sihan Yang,
Yixue Zhou and
Changhai Liang*
Laboratory of Advanced Materials & Catalytic Engineering (AMCE), School of Chemical Engineering, Dalian University of Technology, Panjin 124221, China. E-mail: changhai@dlut.edu.cn; Fax: +86-411-84986353; Tel: +86-411-84986353
First published on 6th January 2022
In this work, a series of colloidal gold nanoparticles with controllable sizes were anchored on carbon nanotubes (CNT) for the aerobic oxidation of benzyl alcohol. The intrinsic influence of Au particles on the catalytic behavior was unraveled based on different nanoscale-gold systems. The Au/CNT-A sample with smaller Au sizes deserved a faster reaction rate, mainly resulting from the higher dispersion degree (23.5%) of Au with the available exposed sites contributed by small gold particles. However, monometallic Au/CNT samples lacked long-term stability. CeO2 was herein decorated to regulate the chemical and surface structure of the Au/CNT. An appropriate CeO2 content tuned the sizes and chemical states of Au by electron delivery with better metal dispersion. Small CeO2 crystals that were preferentially neighboring the Au particles facilitated the generation of Au–CeO2 interfaces, and benefited the continuous supplementation of oxygen species. The collaborative functions between the size effect and surface chemistry accounted for the higher benzaldehyde yield and sustainably stepped-up reaction rates by Au-Ce5/CNT with 5 wt% CeO2.
Supported Au nanoparticles (Au NPs) with outstanding surface chemistry were preferentially focused due to their excellent selectivity for heterogeneous oxidations compared with other precious metals.6,7 However, the conversion and stability of gold catalysts during aqueous reaction still need efficient promotions. In fact, one of the accepted strategies will be optimizing the sizes and distribution of Au NPs to maximally obtain coordination-unsaturated Au sites,8,9 only if the reaction is structure–sensitive with a clear size effect. Although such topic aroused more and more research interest, the main discussion on the surface- and structure-effect of gold catalysts is still in dispute for the aerobic oxidation of BnOH. Zhu et al.10 have encapsulated small Au NPs (5 nm) in the zirconium-based metal organic framework (UIO-66), and the hydrophilic surface of UIO-666 with a high dispersion of Au particles was suggested to be responsible for the good stability and reusability. Haider et al.11 used Au/TiO2 and Au/CeO2 as models, and the Au catalyst with average size of 6.9 nm displayed superior activity compared with other samples (1.3–11.3 nm). However, the intrinsic activity that could be revealed by turnover frequency (TOF) was not clearly compared, and the intrinsic influences of the sizes and structure were still unknown. Xu et al.12 studied the influences of the sizes and types of Au clusters in Aun/LDH (n = 25, 38, ∼127) for aerobic BnOH oxidation. Although the Au38/LDH displayed higher TOF value, the TOFs of Au clusters with different sizes were very close in the range of 1464–1605 h−1. On the other hand, Olmos et al.13 claimed that the order of magnitudes of TOF could be significantly influenced by the thermal treatment, support, and especially the type of active sites. The TOFs of different Au–Pd/CeO2–ZrO2 samples increased to about 18-fold as the particle sizes grew from 1.7 to 2.0 nm, even if their metal dispersions were identical (1.6 wt%). Hong et al.6 investigated the Au–Pd bimetallic catalysts for the selective oxidation of BnOH. However, the BzH yields of Au–Pd catalysts proved to be irrelevant with the bimetallic particle sizes. Larger Au–Pd particles (15.9 nm) were also able to efficiently convert the BnOH molecules. The reported literature affirmed the essential responsibility of the constructed bimetallic Au–M(O)x interface (M could be Pd, Pt, Ag, Cu, Ce, Fe, Mg, etc.) for the high-efficiency gold catalysts.14–16 However, the precise understanding of the size- and structure-effect for BnOH oxidation based on bimetallic Au–M(O)x sites turned out to be an extremely complicate task due to the mingling of hybrid sites. In a word, a controversial discussion exists either due to the interferences by the strong interaction between the Au-secondary metal/support, or the multiple parameters induced by the complex system. The understanding of efficient catalysts for aerobic BnOH oxidation should be carried out preliminarily on the monometallic Au catalysts, and the catalytic system affected by a well-constructed interface can thus be boldly explored.
In order to avoid other influencing factors caused by the pre-treatment, strong metal support interaction (SMSI), or depositing process, the support should be properly chosen with the available synthesis strategy.17–19 Nano carbon materials, e.g., carbon nanotubes (CNT), carbon spheres (CS), carbon fibers (CF) and graphene, are becoming the most popular alternative supports due to their abundant earth-reserves and easily controlled surface chemistry.20,21 Most important of all, strong synergy is hardly formed between gold and carbon (e.g., CNT) unless special treatment was processed.22 The weak interaction between gold and CNT acts as a double-edged parameter. It indeed results in the inferior activity, but availably eliminates the interference of SMSI effect during research work. Herein, in this work, monometallic Au catalysts were preliminarily used as the simple model to understand the size and structure effect on the performances of BnOH oxidation. Colloid immobilization method by different coupling agents was applied to obtain gold with controllable size distributions. The structure–sensitivity and the structure–performance relationship were firstly unraveled by the combination of both turnover frequency (TOF) and apparent reaction rate based on monometallic gold samples. Considering the insufficient stability of the monometallic gold catalyst, the CeO2 dopant was subsequently doped in the catalysts to remedy the oxygen store/releasing ability and distribution of active sites by controlling the metal contents. The construction of the Au–CeO2 interface, as well as their influences and contribution to the catalytic behavior of aerobic oxidation, were analyzed and correlated.
Fig. 1 TEM images and the size distributions of: (a1) TEM images of fresh gold colloid, (a2–a3) Au/CNT-A, (b1–b3) Au/CNT-TH, (c1–c3) Au/CNT-TL and (d1–d3) Au/CNT-Na. |
The TEM images of the Au/CNT-TH and Au/CNT-TL samples using tannic acid as a stabilizer are shown in Fig. 1(b1–b3) and (c1–c3). The average sizes of the Au NPs in the Au/CNT-TH and Au/CNT-TL samples are 9.1 and 14.4 nm, respectively, which are larger compared with those in Au/CNT-A. Particles in Au/CNT-Na are even larger and randomly dispersed (Fig. 1(d1–d3)). The statistical result suggests that the average size of Au/CNT-Na is 21.9 nm in Au/CNT-Na based on more than 200 particles.
The crystal structure of different gold catalysts was further detected by the XRD patterns (Fig. 2a). The amorphous carbon was confirmed by the broad and intensive peak at 26.6° (PDF#41-1487), corresponding to the (002) crystal plane of graphite. Several diffraction peaks at 38.2°, 44.4°, 64.6° and 77.6° correspond to the (111), (200), (220) and (311) crystal planes of gold (PDF#4-784),23 suggesting the presence of Au NPs in all samples. The average sizes of Au NPs are calculated to be 5.8 nm, 9.4 nm, and 16.2 nm and 17.3 nm for the Au/CNT-A, Au/CNT-TH, Au/CNT-TL, and Au/CNT-Na samples based on the Au(111) face. The XRD results are generally consistent with the statistical results of TEM.
Fig. 2 (a) XRD patterns, (b) Raman spectra and (c) the ID/IG value changes along with the particle sizes of different Au/CNT catalysts. |
The direct consequences of metal deposition and thermal treatment on the carbon materials are the co-generation of surface defects. Herein, Raman spectra of different samples are displayed in Fig. 2b. Two intensive peaks are observed in the range of 1700–1100 cm−1. The peak at 1343 cm−1 labeled as D is attributed to the structural defects and the partially disordered structure of the sp2 carbon. The Raman peak at 1573 cm−1 is assigned to the G band, which is related with the degree of graphitization.24 The ID/IG value calculated based on the deconvolution of Raman spectra directly reflects the formation degree of the surface defects. The ID/IG value of the purified CNT is only 0.94. The deposition of Au NPs caused the higher ID/IG value in the range of 1.40–1.57. The variation of the ID/IG value changes, along with the average particle sizes by TEM results, is displayed in Fig. 2c. The much higher value of ID/IG in the Au/CNT-A and Au/CNT-TH samples indicates the easier generation of abundant surface defects on carbon after the loading of smaller gold particles.
In fact, compared with the freshly dried samples at 60 °C, the series of Au/CNT samples lost about 5–8% weight mass after calcination, mostly attributed to the surface adsorbed moisture. The surface evolution and generation of defects simultaneously occurred during the thermal treatment,25,26 with the CNT structure being well-maintained, as shown by the TEM images.
In the XPS spectra of the Au 4f core level (Fig. S1†), typical Au0 species with binding energy of 84.2 eV and 87.7 eV are observed in all of the catalysts, and belong to the Au 4f5/2 and 4f7/2 regions.27,28 The surface weight ratio of Au/C based on XPS data in Au/CNT-Na is only 2.7 wt% and is much lower than the other gold samples (3.5–4.2 wt%). Considering XPS as a technique detecting the upper layer surface of 5–10 nm, most of the Au signals inside the big Au NPs are beyond the detection limit of the XPS, causing the much lower ratio of Au/C in the Au/CNT-Na sample.
The reaction performance of the typical Au/CNT-A at different temperatures was also detected to understand the influences of the reaction temperature (Fig. 3b). It is suggested that only 48% BnOH is transformed at 40 °C. The rising reaction temperature leads to the increasing BnOH conversion to about 80% at 70–80 °C. However, the BzH selectivity decreases from 83% at 40 °C to 70% at 80 °C due to the facile production of benzaldehyde (BzH) by excessive oxidation. The apparent reaction rates by different Au/CNT samples are calculated (Fig. 3b) at lower temperature (40 °C) to limit the BnOH conversion as less than 20%, and other reaction conditions are listed in Table S1.†
The reaction rate changes in the range of 5–15 mmol gAu−1 h−1 by different gold catalysts. The apparent reaction rate and catalytic conversion of BnOH by Au/CNT-A and Au/CNT-TH with smaller particles are indeed superior to the other samples. As the particle sizes become larger, the apparent reaction rates by the Au/CNT-TL and Au/CNT-Na samples are sharply reduced to 8.4 and 5.3 mmol gAu−1 h−1, respectively. The turnover frequency (TOF) based on per Au atom per hour in different catalysts were also calculated (Fig. 3c & Table S1†). The TOFs in the range of 5.83–1.63 × 102 h−1 oppositely change with the growth of the Au particles. The TOF by Au/CNT-A (4.9 nm by TEM) is about 3.6-fold of that for Au/CNT-Na (21.9 nm). Thus, the particle sizes greatly influence the number of converted BnOH molecules by a single Au atom, suggesting a typical size-sensitive reaction using gold catalysts. Under such circumstance, it can be imagined that the distinctive catalytic behaviors should be mainly induced by the available exposure of active gold sites. Smaller particles have larger surface area and higher percentage of exposed unsaturated Au atoms (surface distribution degree in Table S1†), which are essential for the transformation of BnOH to BzH.
The Au/CNT-A with better catalytic behavior was tested by the circular reaction (Fig. 4a). However, the Au/CNT-A sample gradually encountered deactivation during the circular tests. The conversion of BnOH greatly decreased from 44% to 23% after the 4th reaction cycle. It was previously suggested that a strong interaction between Au and the carbon support was difficult to form unless a supplementary surface property or other chemical element existed.29 To improve the reactivity and stability under mild conditions, ceria was added as a doping element considering the famous oxygen redox property engaged by CeO2 and the easily formed contact between gold and reducible metal oxide. Au/CeO2 (1.5 wt%) and CeO2/CNT as references were first prepared for the blank tests.
The BnOH conversion by Au/CeO2 at 80 °C was 40.0% with 84% BzH selectivity, which is inferior to the series of Au/CNT samples. CeO2/CNT displayed poor activity with less than 10% conversion of BnOH under the same condition. Surprisingly, the reactions by typical Au-Cex/CNT samples can be efficiently catalyzed under even milder conditions at 40 °C. As shown in Fig. 4b, the catalytic performances parabolically change with the ceria contents. As the CeO2 contents increase from 0 to 5.0%, the conversion of BnOH significantly increases. It reaches 79% BnOH conversion with 85% BzH selectivity by Au-Ce5/CNT under 40 °C. A further increase of the CeO2 content causes the obvious decrease of both BnOH conversion and BzH selectivity by the Au-Ce7.5/CNT and Au-Ce10/CNT samples. In order to understand the influence of ceria on the stability of the Au-Ce5/CNT catalyst, the circular reaction was carried out, as shown in Fig. 4c. The catalyst was generally stable during the five-reaction cycles. Only a slight decrease of the BnOH conversion from 79% to 76% was observed with the selectivity of BzH increasing from 85% to 88%. The decoration of ceria greatly enhanced both the catalytic activity and the stability of Au-Ce5/CNT during the repetition test.
Fig. 5 XRD patterns (a) & H2-temperature programmed reduction curves (b) of the catalysts with different CeO2 contents. |
The purified CNT displays a small asymmetric reduction peak centered at about 600 °C, which should be attributed to carbon methanation in the presence of H2.26 The deposition of Au NPs facilitates the methanation of CNT as the reduction peak area further increases in Au/CNT-A. The reduction of the gold species should be located at a lower position (50–150 °C), which is absent in the detected sample, suggesting that most of the Au species on the surface have been reduced. After CeO2 doping, the peak area sharply rises with higher CeO2 contents. Additional reduction peaks in the range of 250–500 °C appear in accordance with the reported reduction peaks of the CeO2 nanoparticles at 300–600 °C.32 As the CeO2 content rises, the peak maximum shifts to higher temperature, especially in the Au-Ce7.5/CNT and Au-Ce10/CNT samples. Combining the XRD patterns of different samples, the higher reduction temperature should be caused by the large crystal sizes of CeO2. Regardless, the CeO2 doping results in a more intense peak area, indicating the enhancement of the reducibility and redox capacity of the gold catalysts. It is further correlated with the ability to activate/supply active oxygen and lays great importance on the catalytic performances for oxidation. By comparing the H2 consumption of Au-Cex/CNT with Au/CNT-A, the peak area obviously exceeds the stoichiometric value needed for the reduction of CeO2. It is indicated that the anchored CeO2 also enhances the methanation of CNT at higher temperature. Interaction should occur between the dispersed CeO2 crystals and CNT support.
To obtain more surface information on the CNT structure, the XPS spectra in the O 1s region were obtained and are illustrated in Fig. 6. The O 1s spectra is deconvoluted into three overlapped peaks located at 531.4, 532.4, and 533.8 eV, corresponding to the CO, O–CO and C–O groups, respectively.33 Compared to the oxygen content of CNT (O/C atomic ratio of 1.8%, Table S2†), the O/C ratio in Au/CNT-A is 2.3 at%. After ceria decoration, an additional peak around 529.8 eV remarkably appeares in the Au-Cex/CNT samples. It should be ascribed to the lattice oxygen.34,35
Fig. 6 XPS spectra of the O 1s core level by the (a) Au/CNT, (b) Au-Ce2.5/CNT, (c) Au-Ce5/CNT and (d) Au-Ce10/CNT samples. |
As the ceria contents increase, the total O/C ratios increase from 2.3% in Au/CNT-A to 4.9–7.6% in the Au-Cex/CNT samples. The percentages of the lattice oxygen account for 1.3–2.9% in the gold catalysts with different CeO2 contents. The results of the O 1s spectra are in accordance with the H2-TPR results, showing that the oxygen supply ability is obviously promoted due to the existence of ceria and supplementation of lattice oxygen.
The XPS spectra of the Au 4f core level by Au/CNT-A and Au-Cex/CNT are illustrated in Fig. 7. As mentioned above, only metallic Au0 exists in the monometallic Au/CNT-A. Different from Au/CNT-A, positively charged Au species (Auδ+) are generated and detected in the series of Au-Cex/CNT samples, which are 5%, 10% and 9% in the total gold species of the Au-Ce2.5/CNT, Au-Ce5/CNT and Au-Ce10/CNT samples, respectively. Auδ+ was also reported to exist in metal oxide promoted gold catalysts, and was beneficial for heterogeneous reactions.36 It is inferred that the specific interaction and interfaces have been formed between gold and ceria. In the series of Au-Cex/CNT samples, connection between Au and the ceria-decorated CNT likely happenes and electrons are delivered from gold to ceria to give the more positively charged Auδ+ species.
Fig. 7 XPS spectra of the Au 4f core level by the (a) Au/CNT, (b) Au-Ce2.5/CNT, (c) Au-Ce5/CNT and (d) Au-Ce10/CNT samples. |
The TEM images of Au-Ce5/CNT are shown in Fig. 8. Small Au NPs around 3.8 nm are highly dispersed in the catalyst. It is difficult to directly identify the location of CeO2 due to the poor contrast of the TEM images in low magnification. In this case, high-resolution TEM images were carried out. The Au particles and ceria crystals can be identified by counting the inter-planar distances. Both typical lattice distances of the Au(111) phase and ceria can be frequently observed on the surface. A small amount of isolated ceria is also present, while most of the Au NPs are adjacent to the ceria crystals, either due to the reported selective adsorption/deposition between metal (oxides) or the ubiquitous dispersion of small ceria crystals.37 The HAADF-STEM elemental-mapping of the Au-Ce5/CNT also proved that the Ce signals were uniformly dispersed on the surface of CNT (Fig. S2†). It is also interesting to note that mutual interfaces were more frequently built and detected between the Au(111) and CeO2(400) crystal phases. The construction of the Au–CeO2 interface facilitates the oxygen supply from the CeO2 near the Au NPs and accelerates the oxidation rate of BnOH.
The major surface and chemistry factors influencing the catalytic behaviors of Au catalysts are now well-known and can be summarized as follows: (i) the particle sizes of gold, and (ii) the oxygen activation and redox properties enhanced by the additional metal oxide. After ceria decoration, both reaction rates at 40 °C and 50 °C by typical Au-Cex/CNT (x = 2.5, 5, 10) samples were calculated. The reaction rates by different Au-Cex/CNT samples were in the range of 9.4–15.7 mmol gAu−1 h−1 at 40 °C, which grew in inverse proportion to the average particle sizes – either by XRD or TEM results – in the Au/CNT and the Au-Cex/CNT systems (Fig. 9 & Table S3†). The regular decrease of reaction rates was also observed with the increasing Au sizes. Compared with the reaction rate of Au/CNT-A at 40 °C (7.6 mmol gAu−1 h−1), the reaction rates of the Au-Cex/CNT system with similar sizes of particles were greatly promoted, which should be a combined effect from multiple parameters beyond the size effect.
In fact, one problem with using monometallic gold catalysts for the selective oxidation of BnOH is that the adsorption/dissociation of both O2 and BnOH molecules are indispensable on the surface of the monometallic gold catalyst. Herein, the competitive adsorption between BnOH and O2 during the reaction was frequently reported, following the Langmuir–Hinshelwood model.38 The sizes of the Au NPs become essential since smaller particles exposes more gold sites to activate/dissociate reactant molecules with higher TOF. H2-TPR results reflect the much better redox properties of the series of Au-Cex/CNT after ceria doping, either due to the supplementation of the CeO2 lattice oxygen or O2 dissociatively adsorbed on ceria nearby Au NPs. An even higher CeO2 content changes the surface chemistry, however, at the cost of forming larger Au NPs and separated ceria crystals. Therefore, the appropriate CeO2 content is significant for the oxidation of BnOH. A high dispersion of CeO2 around the Au NPs was confirmed by XRD and TEM in the Au-Ce5/CNT sample. The close contact between gold and ceria provides new reaction sites at the interfaces, and the active oxygen species during the reaction can be continuously supplied.
Under such circumstance, Au NPs with smaller sizes provide the effective transformation of BnOH with a higher number of available exposed active sites, while the additional ceria promotes the activation/supplementation of the oxygen species during the reaction. The prerequisite for the successful and fast transformation from BnOH to BzH can thus be achieved by the current system.
Based on the above discussion, the available reaction pathway by the ceria-promoted gold catalyst is displayed in Scheme 1. Molecular oxygen was suggested to take part in the reaction by forming a hydroxide or hydroperoxo-species on the surface of the metal oxide (e.g., CeO2) instead of directly dissociating to oxygen atoms,39,40 which was suggested to be beneficial for abstracting the β-hydride of the alcohol. H2O2 was also reported to be detected during the oxidation of BnOH, especially if there was an active metal (oxide) as the doping element near the Au NPs.41,42
During the reaction, the ceria composition near the small Au NPs is responsible for supplying the active oxygen species ˙O2−, by either supplementation from the lattice oxygen or adsorption/dissociation of gaseous molecular oxygen. The proton abstraction of molecular BnOH subsequently occurred by forming –OOH on the surface of the neighboring ceria. The deprotonated BnOH* is adsorbed on the surface of gold with positively charged Auδ+ (as detected by XPS spectra) to form an alkoxide intermediate after step I.43 The β-H in BnOH* is then bonded with gold atoms (step II) and is eliminated to produce the gold-hydride intermediate during step III. BzH is simultaneously released, leaving the proton occupying the surface of Au NPs. The cleavage of C–H was reported to be the rate-determining step for BnOH oxidation,44 which should be preferentially operated by unsaturated sites. Herein, samples with smaller sizes were related with the better yield of BzH. The initial surface of the ceria-promoted gold catalyst can be finally recovered by releasing the H2O2 molecules (step IV). The new circulation was continuously operated until the oxidation process was fulfilled.
The turnover frequency (TOF) of a typical sample was calculated based on the statistical results of the TEM images by the following equation:
The NBnOH denotes the transferred number of BnOH molecules, which was controlled by lowering the reaction temperature (40 °C) and catalyst dosage; t is the reaction time in hour; the NAu is the total number of Au atoms in the catalyst; Dm is the surface dispersion degree of Au, and can be calculated by the equation between the particle area (SNP) and weight (mNP) of one Au NP, as well as the sectional area of a Au atom (SAu):
Au is the molar mass of Au (197 g mol−1) and NA is the Avogadro constant.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d1ra07686h |
‡ The authors contributed equally to the work. |
This journal is © The Royal Society of Chemistry 2022 |