Yang Jiaoab,
Shenghan Zhang*ab and
Yu Tanab
aHebei Key Lab of Power Plant Flue Gas Multi-Pollutants Control, Department of Environmental Science and Engineering, North China Electric Power University, Baoding, 071003, China. E-mail: shenghan_zhang@126.com
bEnvironmental System Optimization, College of Environmental Science and Engineering, North China Electric Power University, Beijing, 102206, China
First published on 11th January 2022
Carbon steel is widely used as the piping of the primary heat transport system (PHT) in pressurized heavy water reactors (PHWR). Effects of zinc/aluminum treatment and simultaneous injection of zinc and aluminum on corrosion behavior and semiconductor properties of oxide films formed on carbon steels were characterized by the gravimetric method, potentiodynamic polarization scan, EIS, Mott–Schottky test, SEM, EDS mapping, XPS analysis and photocurrent response measurement. The results showed that all the metal cation ions treatment can improve the corrosion resistance of oxide films in varying degrees. 20 ppb Zn2+ had the greatest enhancement in corrosion resistance, followed by 20 ppb Zn2+ + 20 ppb Al3+. ZnFe2O4, FeAl2O4 and ZnAl2O4 were detected to be new spinel phases generated in oxide films. The oxide films on the surface of carbon steel all demonstrated n-type semiconductor properties. It was worth noting that the total content of manganese and zinc in the oxide film played an important role in the corrosion resistance of carbon steel.
In nuclear power plants, water chemistry of the coolant is carefully monitored and controlled for the integrity of the system structure.7,8 Although CANDU design is significantly different from that of light water reactors (LWR), many materials corrosion and degradation issues are equally important and directly affect the safety of reactor operation. Carbon steel pipes corrode during the high temperature (inlet and outlet temperature being 266 °C to 310 °C) and high pressure in long-time operation. Therefore, to reduce the corrosion of carbon steel and prevent local deposition of corrosion products, an alkaline pH25 °C of 10.2–10.6 is maintained by the addition of lithium hydroxide (LiOH) in the reactor primary circuit.4,9–11
It has been reported that the composition and grain boundaries of alloys could be modified to improve their corrosion resistance.12 Zinc injection technology has been widely used in the primary circuit coolant of nuclear power plants. It is generally considered that the addition of zinc into the coolant can retard the corrosion rate of metal materials and reduce the buildup of radiation field and the occupational radiation dose.13
Many studies have reported that the compact oxide layer and high corrosion resistance of carbon steel could be obtained due to the generation of zinc ferrite (ZnFe2O4) oxide. Sawicki's research identified the effects of 15–60 ppb soluble zinc on the surface composition of carbon steel in primary-side coolant by using conversion and electron and X-ray backscattering Mössbauer spectroscopy. High electrical resistivity zinc ferrite was formed on coupons when exposed to zinc added solution. A layer of zinc ferrite in the oxide film played an important role in reducing corrosion products release rates.14 Walker Z. H. pointed that in the presence of 15 ppb zinc only a slight reduction was found in corrosion of CS coupons. Moreover, zinc ferrite showed a significantly lower thermal conductivity than without zinc addition and reduced the heat transfer efficiency in the primary circuit.15
However, 64Zn in natural zinc was easily irradiated by neutrons to produce high radioactive 65Zn, expensive depleted zinc was used in nuclear power plants. 27Al is a stable nuclide and have no radioactive. Aluminium ion is a good corrosion inhibitor which has been widely applied in industrial cooling water. Previous studies have addressed the influence of zinc and aluminium simultaneous injection on corrosion behaviours of stainless steels in simulated PWR primary circuit environments.16–18
The aim of this study was to evaluate the effect of zinc and/or aluminum added into simulated primary circuit coolant of heavy water reactors. The oxide films on carbon steels were formed in high temperature and high pressure solutions. After oxidation for 168 h, the corrosion behavior and semiconductor properties of samples were analyzed by potentiodynamic polarization scan, electrochemical impedance spectroscopy (EIS), and Mott–Schottky curve. The morphology of carbon steel surface was measured by scanning electronic microscopy (SEM). The composition of oxide films were analyzed by photocurrent response, energy dispersive spectrometer (EDS) mapping and X-ray photoelectron spectroscopy (XPS).
Test solution | Li+ (ppm) | Zn2+ (ppb) | Al3+ (ppb) |
---|---|---|---|
T (blank) | 1 | 0 | 0 |
T (20Zn) | 1 | 20 | 0 |
T (40Zn) | 1 | 40 | 0 |
T (30Al) | 1 | 0 | 30 |
T (20Zn + 20Al) | 1 | 20 | 20 |
Potentiodynamic polarization scan and electrochemical impedance spectroscopy (EIS) were carried out with CHI650D electrochemical workstation of Shanghai Chenhua Ltd at room temperature. Firstly, the open circuit potential (OCP) which unit was volts (V) was measured and monitored. The OCP value was determined in a stable state based on the changes in OCP value were less 10 mV within one minute. The actual entire immersion time from electrode immersion to stability state did not exceed 10 minutes. Then, the scanning range of potentiodynamic polarization were performed from −1.0 V to 0.8 V with respect to OCP at a scan rate of 0.001 V s−1. EIS was measured at OCP with a frequency from 106 Hz to 10−2 Hz with the sinusoidal voltage of ±10 mV on the oxide films. Finally, the electrical parameters and fitting of the spectra were done by an equivalent electrical circuit using ZSimpwin software. Mott–Schottky curve were carried out with PARSTAT2273 potentiostat of Princeton Ltd in three-electrode cell. The potential range of test was −1000 mV to +1200 mV with a potential step of 0.01 V.
The photocurrent responses were performed by focusing a monochromatic modulated light through the quartz window on to the oxide films. A xenon lamp (350 W, Crownetch) with a grating monochromator (1/8 m, CT110, Crowntech) was used as the light source. The wavelength of lights ranged from 200 nm to 800 nm in steps of 10 nm. Before the experiments, the light intensity of different wavelength was measured by connecting a Si-photodiode to a digital ammeter positioned in the same place of the coupon. The photocurrent response value of the oxide films at different wavelength were mathematically transformed to attain the data with the change of photo energy.
The corrosion rate of carbon steel in high temperature solution was calculated by eqn (1):
(1) |
(2) |
Group | Corrosion rate (g mm−2 d−1) | Standard deviation |
---|---|---|
T (blank) | 1.000 | 0.33 |
T (20Zn) | 0.5714 | 0.25 |
T (40Zn) | 0.8333 | 0.49 |
T (30Al) | 0.8571 | 0.21 |
T (20Zn + 20Al) | 0.5238 | 0.24 |
It can be seen from the calculated results that with the injection of zinc and/or aluminum the corrosion rate of carbon steel decreased compared to T (blank). Samples in 20 ppb Zn2+ solution showed better corrosion resistance than that in high concentration of Zn2+. T (20Zn + 20Al) had the slowest corrosion rate (half of T (blank)) which implied the best corrosion resistance of oxide film, but the reduction effect of zinc–aluminum injection was not significant.
OCP (V) | Ecorr (V) | icorr (A cm−2) | |
---|---|---|---|
T (blank) | −0.531 | −0.540 | 5.085 × 10−8 |
T (20Zn) | −0.118 | −0.121 | 4.826 × 10−9 |
T (40Zn) | −0.356 | −0.357 | 1.310 × 10−8 |
T (30Al) | −0.674 | −0.681 | 4.948 × 10−8 |
T (20Zn + 20Al) | −0.348 | −0.349 | 7.035 × 10−9 |
The high corrosion resistance in absence and presence of Zn2+ and Al3+ is attributed to protective nature of the passive film. From the data shown in Table 3, compared with blank group, the lower icorr values for all the oxide samples were indicative of the better corrosion resistance. It was obvious that icorr of T (20Zn) and T (20Zn + 20Al) showed an order of magnitude lower than other groups, and the open circuit potential (OCP) shifted toward to the noble side (−0.118 V and −0.348 V vs. SCE) compared carbon steel in blank group (−0.531 V vs. SCE). However, with sole injection of aluminum, icorr showed little decrease than T (blank), which result in little effect on the improvement of corrosion resistance. Consequently, among the different concentration of solution, 20 ppb Zn2+ was the most effective for improving the corrosion resistance of carbon steel in heavy water reactor water conditions.
EIS measurements were carried out for all samples in 1 ppm LiOH solution at room temperature. The Nyquist, phase angle and Bode plots of oxide films formed on carbon steel coupons in high temperature water with different concentration of zinc and aluminum were shown in Fig. 2(a), (b) and (c) respectively. For clearer comparison, Bode plots at low frequencies were shown in Fig. 2(d).
Two semicircles seen in Fig. 2(a) Nyquist diagram indicated the presence of two time constants attributed to process occurring near oxide/solution interface and oxide/metal interface after carbon steels exposed to high temperature water. The Bode spectra (Fig. 2(c) and (d)) showed a significant increase of impedance modulus at low frequencies after zinc and zinc + aluminum injected in the solution, especially for T (20Zn) which demonstrated the highest value of Z in the lowest frequency. The Bode plots of T (30Al) were almost coincide with T (blank), only a little lower than T (blank) when frequency less than 0.25 Hz, which indicated these two groups had similar corrosion resistance.
Several circuit models were attempted to fit the above experimental data. The best agreement between experimental and fitted data (shown in Fig. 2) was obtained with the equivalent circuit model illustrated in Fig. 3. In the equivalent circuit model, Rs represents the resistance of solution, Rout and Qout are the resistance and constant phase element (CPE) of outer oxide films with respect to the oxide/solution interface, Rin and Qin are the resistance and CPE of inner oxide film the oxide/metal interface. Each parameter of circuit elements was fitted in Table 4.
Group | Rs (Ω cm−2) | Qout | Rout (Ω cm−2) | |
---|---|---|---|---|
Yout (S secn cm−2) | nout | |||
T (blank) | 4.28 × 10−4 | 2.677 × 10−8 | 0.7093 | 6.632 × 103 |
T (20Zn) | 1.63 × 10−5 | 1.866 × 10−8 | 0.7369 | 6.569 × 103 |
T (40Zn) | 2.39 × 10−5 | 1.906 × 10−8 | 0.7355 | 6.770 × 103 |
T (30Al) | 6.78 × 10−4 | 3.589 × 10−8 | 0.6846 | 6.641 × 103 |
T (20Zn + 20Al) | 1.1 × 10−3 | 6.32 × 10−8 | 0.6393 | 1.209 × 104 |
Group | Qin | Rin (Ω cm−2) | |
---|---|---|---|
Yin (S secn cm−2) | nin | ||
T (blank) | 3.789 × 10−5 | 0.7531 | 2.614 × 105 |
T (20Zn) | 8.875 × 10−6 | 0.7434 | 1.145 × 106 |
T (40Zn) | 1.677 × 10−5 | 0.7935 | 6.420 × 105 |
T (30Al) | 4.654 × 10−5 | 0.6382 | 1.206 × 1013 |
T (20Zn + 20Al) | 1.143 × 10−5 | 0.7798 | 1.260 × 1017 |
It was obvious that all ion injection treatments increased the resistance of the oxide films formed on CS showing better corrosion resistance. This behavior was also confirmed in the potentiodynamic polarization measurements. The values of Rin were much larger than Rout in each group and were larger than those of T (blank), which demonstrated the corrosion processing was mainly controlled by the charge transfer at the interface of the inner oxide/metal layer. It was worth noting that the inner resistance increased sharply when Al3+ added into simulated primary circuit water, at the same time the aluminum ion as corrosion inhibitor to improve the corrosion resistance of inner structure of oxide films were verified.
Because of the dispersion effect of electric double layer capacitor, for the description of a frequency independent phase shift between the applied AC potential and its current response, CPE which has non-integer power dependence on frequency, was employed and the impedance of CPE was given by the following equation eqn (3):
(3) |
(4) |
(5) |
MS plots of carbon steel samples with oxide films obtained in different Zn2+ and Al3+ injection conditions were shown in Fig. 4. The test potential was in the range of −1000 mV to +1200 mV and the test solution was 1 ppm LiOH solution at room temperature. The variation of C−2 with the applied potential was typical of an n-type semiconductor. The carrier concentration (Nd) and flat band potential (Efb) calculated were listed in Table 5.
Fig. 4 Mott–Schottky curves of oxide films formed on CS in different Zn2+ and Al3+ injection conditions. |
Group | Semiconductor type | Nd (cm−3) | Efb (V) |
---|---|---|---|
T (blank) | n | 2.10 × 1017 | −0.14 |
T (20Zn) | n | 5.37 × 1016 | −0.43 |
T (40Zn) | n | 3.42 × 1017 | −0.46 |
T (30Al) | n | 1.76 × 1017 | −0.79 |
T (20Zn + 20Al) | n | 1.73 × 1017 | −0.32 |
The Nd of oxide film formed in 20 ppb Zn2+ solution (5.37 × 1016 cm−3) was the lowest among all groups, which was approximately 25.6% of Nd of T (blank) (2.10 × 1017 cm−3). The reduction of the carrier concentration varied in degrees compared to T (blank) after Zn2+ and/or Al3+ injected into high temperature water. Furthermore, the flat band potential (Efb) had a negative shift with all treatment of solution compared to T (blank) (−0.14 V vs. SCE). It has been reported that Zn2+ in the spinel structure can reduce the defects which may inhibit the transportation of ions from the metal to solution and minimize the corrosion rate. From the results in Mott–Schottky tests, it can be concluded that the corrosion resistance and the stability of the passive film was improved, and the improvement may be due to the changes in the composition of oxide films formed on carbon steel in different conditions. In the next parts, the composition was analyzed by different methods.
Fig. 5 SEM images of oxide films formed on CS in different conditions (a) T (blank) (b) T (20Zn) (c) T (40Zn) (d) T (30Al) (e) T (20Zn + 20Al). |
Fig. 6 EDS mapping images of oxide films formed on CS in different conditions (a) T (blank) (b) T (20Zn) (c) T (40Zn) (d) T (30Al) (e) T (20Zn + 20Al). |
The loose surface morphology with flaky crystals can be observed on the carbon steel samples corroded in simulated primary circuit coolant at high temperature without zinc and aluminum (as shown in Fig. 5(a)), which mean CS had poor corrosion resistance in lithium hydroxide solution. The average size of particles was approximately 3.1 μm.
After using zinc and/or aluminum treatment, the surface of oxide films formed on carbon steels displayed different morphologies (as shown in Fig. 5(b)–(f)). The surface became denser and smoother in varying degrees, and at the same time, many regular tetrahedral and octahedral crystals were observed. With the increase of Zn2+ concentration, the surface morphologies were different and the average size of particles were also increased, for which about 1.8 μm in T (20Zn) and 2.4–2.5 μm in T (30Zn) and T (40Zn). Combined with the above electrochemical test results, it was implied that smaller size and denser oxide particles would be useful to improve the corrosion resistance of carbon steel. The average size of particles in T (30Al) were 1.5 μm and the surface of oxide films seems denser than T (20Zn), however the corrosion resistance was not significantly improved due to the results in potentiodynamic polarization analysis. It may be due to different composition of oxide films when Zn2+ or Al3+ injected into solution.
The EDS mapping of Zn and Al were detected in oxide films (as showed in Fig. 6(b)–(f)), indicating that Zn2+ and Al3+ in the solution reacted with carbon steels in high temperature conditions. Zinc and aluminum appeared simultaneously in the oxide films of T (20Zn + 20Al) could be attributed to the replacement of part of zinc by aluminum so as to participate in the formation of oxide films. It can be speculated according to the previous researches,18,22 zinc ferrite (ZnFe2O4), FeAl2O4 and zinc aluminate (ZnAl2O4) were generated in the treatment of zinc, aluminum and zinc + aluminum respectively, which changed the corrosion resistance of carbon steels.
Atomic (%) | ||||
---|---|---|---|---|
T (blank) | T (20Zn) | T (40Zn) | T (20Zn + 20Al) | |
O | 49.14 | 51.54 | 50.41 | 40.62 |
Fe | 33.70 | 26.63 | 29.37 | 36.35 |
Mn | 17.16 | 12.46 | 12.15 | 15.9 |
Zn | — | 9.37 | 8.06 | 4.92 |
Al | — | — | — | 2.2 |
It has been reported that the peak of Fe 2p3/2 and Fe 2p1/2 for iron oxides were 710.6–711.2 eV and 723.2–724.8 eV, respectively. The existence of satellite peak located at 719 eV and 733 eV indicated the Fe3+ in oxide films. In general, the peak area of iron was the maximum among the metal elements, that is, iron was the main component in the oxide film. Considering the experimental condition and reaction process, it was judged that iron oxides (FeO, Fe2O3 and Fe3O4) are the main substances in T (blank). With the addition of Zn2+ and/or Al3+ the ratio of satellite peak increased, the content of Fe3+ increased, it may be accompanied by the generation of ZnFe2O4.23,24
The Mn2p spectra consisted of Mn2p3/2 (∼641 eV) and Mn2p1/2 (∼652 eV) with an additional satellite peak at approximate 646–647 eV, which confirmed the presence of Mn2+ state (MnO or MnFe2O4) in the oxide films.25 According to the XPS survey scan of each specimen in Table 6, after Zn2+ added into solution, the percentage of Mn decreased from 17% to 12%, which may be due to the replacement of Mn2+ (MnFe2O4) by Zn2+ (ZnFe2O4).
Fig. 7(c) showed the XPS spectra in the Zn2p region for samples, zinc species could be detected in the oxide film in zinc and zinc–aluminum treatment groups. The Zn2p core level spectrum for oxide films showed a doublet, whose peak at the binding energy of ∼1022 eV and ∼1041 eV. The Zn2p3/2 and Zn2p1/2 binding energy positions revealed the oxidation of Zn atoms and Zn2+ chemical state, which may be ZnO and some zinc-containing spinel oxides. The Zn2p1/2 at 1044.8 eV in spectra was in great agreement of the value of ZnAl2O4 in database, indicating the generation of ZnAl2O4 in T (20Zn + 20Al).
From the spectra of Al2p, aluminum was detected in the oxide film of T (20Zn + 20Al) according to the peak at ∼74.1 eV, which proved the form of Al3+ and the substance may be Al2O3 (74.1 eV) and ZnAl2O4 (74.0 eV).26,27 The O1s signal can be fitted with two peaks, respectively due to lattice O2− (529.84 eV) and surface-adsorbed oxygen ions (532 eV). Moreover, it has been reported that ZnO has an unusual O1s spectrum with two peaks possibly indicating either Zn(OH)2 or oxygen vacancies.28
Photocurrent response tests of the oxide film formed on carbon steel were measured to further probe the effects of zinc and aluminum injection on the composition of the oxide film in primary circuit water of heavy water reactors. Fig. 8 presented the photocurrent response spectrums of oxide films formed in different conditions. All the spectrums exhibited the property of n-type semiconductor according to the positive value of photocurrent, these were in consistent with the results of Mott–Schottky tests above. The photocurrent in Fig. 8(a)–(c) increased with the increase of potential and a highest positive peak can be seen at 410 nm. It was shown obviously in Fig. 8(d) that the values of photocurrent in T (30Al) and T (20Zn + 20Al) was much smaller than those of T (20Zn). For implantation of different ions, the photocurrent value fluctuated with the change of wavelength and difference between peaks and valleys were present.
Fig. 8 Photocurrent response spectrum of oxide films formed on CS in different conditions (a) T (20Zn) (b) T (30Al) (c) T (20Zn + 20Al) (d) 0 V vs. SCE for different conditions. |
In order to explore the composition of oxide films formed on carbon steel samples, the band gap energy (Eg) of different semiconductor materials was calculated by eqn (6):29–32
(6) |
Fig. 9 The distribution of light intensity at the position of the working electrode in different wavelength. |
Fig. 10 (iph·hv/I0)1/2 via photo energy for oxide films formed on CS in different conditions. (a) T (20Zn) (b) T (30Al) (c) T (20Zn + 20Al) (d) T (blank). |
Substance | Fitting Eg (eV) | Reference Eg (eV) | |||
---|---|---|---|---|---|
T (20Zn) | T (30Al) | T (20Zn + 20Al) | T (blank) | ||
FeO | 2.4 | 2.4 | 2.4 | 2.3–2.4 | 2.3–2.4 |
Fe2O3 | 2.2 | 2.1 | 2.2 | 2.1–2.2 | 2.1–2.2 |
ZnFe2O4 | 1.8 | — | 1.8 | — | 1.8–1.9 |
ZnO | 3.2–3.6 | — | 3.2–3.6 | — | 3.2–3.6 |
ZnAl2O4 | — | — | 3.85 | — | 3.8–3.9 |
FeAl2O4 | — | 1.78 | 1.78 | — | 1.78 |
MnO | 3.9–4.0 | 4.0 | 3.6–4.0 | 3.6–4.0 | 3.6–4.0 |
MnFe2O4 | 1.76 | 1.76 | 1.76 | 1.76 | 1.76 |
Combined with the EDS mapping and XPS results shown in Fig. 6(a), iron oxides were the main corrosion products in T (blank) and the atomic percentage ratio of Fe/O was close to 0.7, which implied the substance may be the mixture of magnetite (Fe3O4), hematite (Fe2O3) and FeO. In addition, due to the presence of manganese in carbon steel matrix, MnO and MnFe2O4 were also formed in high temperature environment. With the injection of Zn2+ into LiOH solution, FeO, Fe2O3, MnO, ZnO and ZnFe2O4 were the main composition of oxide films formed on carbon steel samples. It has been confirmed that ZnFe2O4 has low solubility and Gibbs free energy and could be preferentially formed in high temperature water and deposited on the surface of metal materials.44 Therefore, samples in T (20Zn) showed superior corrosion resistance. When the solution only had aluminum ions, FeAl2O4 was generated in oxide films. After Zn2+ and Al3+ simultaneously injected in solution, a new substance of ZnAl2O4 was formed in the oxide film, which were considered to improve the stability and corrosion resistance of carbon steels.
Morphology analysis (SEM images) of different ions injection displayed different surface of oxide films but were more compact compared with T (blank). According to the EDS mapping, XPS results and photocurrent response data, it was assumed that MnFe2O4, ZnFe2O4, FeAl2O4 and ZnAl2O4 were generated in the oxide films. Therefore, the corrosion resistance of oxide films formed on carbon steels can be improved by modifying the composition through metal cation ions added into primary circuit coolant in heavy water reactors.
Based on the equivalent circuit model in Fig. 3, the mathematics expression of the impedance of electrode system could be written as eqn (7):
(7) |
The values of nout and nin in the range of 0.5–1 were associated to the heterogeneity and complexity of electrode surface.45 The n value was away from 1 which indicated the presence of a non-homogeneous surface of the oxide film. Data from Fig. 2(c) showed the linear slope of was close to −1, which implied the typical capacitive behavior of passive films in all treatments of carbon steels. Oxide films formed in the presence of Zn2+ and/or Al3+ showed increased capacitive loop which could be related to increase in protectiveness of oxide.46 At low frequencies, the phase angle increased also implied the increment of capacitance. Moreover, the resistance Rin corresponding to the oxide/metal interface increased to 1.26 × 1017 Ω cm−2 and nin value of 0.7798 indicated that the thickening of the oxide film improved the film passivity in T (20Zn + 20Al). It was speculated that the composition of the oxide film has been changed after aluminum ion implantation, but this composition has little contribution to improving the corrosion resistance of carbon steel in primary circuit water of CANDU.
Zinc ferrite (ZnFe2O4), manganese ferrite (MnFe2O4), hercynite (FeAl2O4) and zinc aluminate (ZnAl2O4) are common spinel with the structure of one-eighth of the tetrahedral and one-half of the octahedral interstices filled by cations. Without zinc treatment, magnetite (Fe3O4) and MnFe2O4 formed on the surface of carbon steels. After zinc injected into primary circuit coolant, along with the Fe3+ and Mn2+ ions at tetrahedral sites were progressively replaced by Zn2+, spinel-type oxide of ZnFe2O4 were generated. With only Al3+ in high temperature solution, spinel-structure FeAl2O4 formed on carbon steels. When zinc and aluminum were simultaneously injected, Zn2+ replaced Fe2+ of FeAl2O4 and Al3+ replaced Fe3+ of ZnFe2O4 and preferentially produced ZnAl2O4. The corrosion resistance of carbon steel was significantly enhanced because of the generation of ZnFe2O4 with zinc treatment.
Obviously, although the content of manganese in carbon steel was not too much compared to iron, the manganese oxide and manganese ferrite formed in high temperature water environment also changed with the injection of Zn2+. Cao et al. point out that the difference in deoxidization degree played an important role in the corrosion resistance of carbon steel. The inclusion of potato-like manganese oxide and olive-like sulfide in boiling steel was the reason for its weaker pitting induction sensitivity and lower pitting corrosion growth rate.47 Moreover, manganese used in steel have higher affinities for oxygen than iron. It is clear that even though small amounts of these elements are present in the steel they still have a higher affinity for oxygen than iron.48 In this study, the changes in the total content of manganese and zinc in oxide films based on XPS results were analyzed deeply. Fig. 11 showed the relationship between corrosion current density (icorr) and the content of Mn + Zn. In T (20Zn) the total content of Mn and Zn reached the highest value (21.83%), and at the same time the corrosion current density behaved the lowest value which indicated the best corrosion resistance among different ion concentration treatments. Therefore, for enhance the corrosion resistance and improve the stability of carbon steel, suitable concentration Zn2+ was worth noting, but not as much as possible.
Compared with T (blank), all the implantation can reduce corrosion rate of carbon steels. The oxide film on the surface of carbon steel all behaved n-type semiconductor properties. For different Zn2+ and Al3+ concentration, T (20Zn) and T (20Zn + 20Al) behaved denser surface and better corrosion resistance than other groups. New spinel phases of ZnFe2O4, FeAl2O4 and ZnAl2O4 formed in oxide films enhance the stability and corrosion resistance of carbon steels. In consequence, the oxide film formed with 20 ppb Zn2+ had the highest total content manganese and zinc, the lowest corrosion current density and the best corrosion resistance. Compared with T (20Zn), zinc–aluminum simultaneous injection treatment can also enhance the corrosion resistance to a greater extent, but the effect was not much different than that of zinc injection alone.
This journal is © The Royal Society of Chemistry 2022 |