Wei Liua,
Masao Kamikoa,
Ikuya Yamadab and
Shunsuke Yagi*a
aInstitute of Industrial Science, The University of Tokyo, 4–6–1 Komaba, Meguro-ku, Tokyo 153–8505, Japan. E-mail: syagi@iis.u-tokyo.ac.jp
bDepartment of Materials Science, Graduate School of Engineering, Osaka Prefecture University, 1–1 Gakuen-cho, Naka-ku, Sakai, Osaka 599–8531, Japan
First published on 21st March 2022
The oxygen evolution reaction (OER) is crucial in water splitting for hydrogen production. However, its high over-potential and sluggish kinetics cause an additional energy loss and hinder its practical application. The cobalt spinel oxide Co3O4 exhibits a high catalytic activity for the OER in alkaline solutions. However, the activity requires further enhancement to meet the industrial demand for hydrogen production. This paper presents an electrochemical deposition method to obtain cobalt oxides with a controllable crystallinity on carbon paper (CP). Usually, cobalt oxides grown on CP have a Co3O4 spinel oxide structure. The self-supported Co3O4/CP exhibited a considerable catalytic activity for the OER. When a VS2 layer grown on the CP beforehand by a hydrothermal method was used as substrate, the deposited cobalt oxides were in an amorphous state, denoted as CoOx/VS2/CP, which exhibited a higher OER activity and better stability than those of Co3O4/CP. The enhancement in the catalytic activity was attributed to the mixture formation of different types of cobalt species, including Co3O4, CoO, Co(OH)2, and metallic Co, because of the reduction by VS2. We also clarify the significance of the crystallinity of cobalt oxides in the improvement in the OER activity. This process can also be applied to the direct formation of other types of self-supported oxide electrodes for OER catalysis.
3d transition-metal oxides, as promising candidates, exhibit high OER activities. However, their activity still cannot meet the demand for industrial production of hydrogen. Extensive studies have been carried out to enhance and analyze the catalytic activities of 3d transition-metal oxides for the OER.9–12 For example, Mefford et al. observed the surface of Co(OH)2 under OER conditions using operand microscopy and reported that the OER proceeds mainly at the edge facets of Co(OH)2.13 The edges exhibited a higher OER activity than that at the grain interior of Co(OH)2. Koza et al. synthesized both crystalline and amorphous cobalt oxides by an electrodeposition method and demonstrated that the amorphous cobalt oxide exhibited a higher catalytic activity than that of the crystalline Co3O4.14 Therefore, the amorphization of cobalt oxides is expected to yield a higher activity, but the mechanism is still unclear.
On the other hand, modification with sulfides reduces the resistance in OER catalysis of transition-metal oxides. For example, Kim et al. reported that a Co3O4/MoS2 heterostructure exhibited a considerably higher OER catalytic activity than that of the simple Co3O4.15 They reported that Co3O4 and MoS2 underwent electron transfer at the heterogeneous interface, modulating the adsorption energy of oxygen-containing species on the oxide surface, which led to an OER enhancement. Jiang et al. reported that a double exchange interaction in the spinel oxide structure was ignited by constructing a heterostructure of MoS2 and Fe-doped NiCo2O4.16 Both oxygen vacancies and electronic state transitions activated this effect through the heterostructure between the oxide and sulfide. These heterostructure materials can be synthesized by various methods, such as sol–gel synthesis, solid-state synthesis, electrodeposition, and coprecipitation synthesis.17–19 Among them, electrodeposition can be used to precisely adjust the catalyst loading mass on the substrate surface by controlling the electric quantity. It is also ideal for construction of heterostructures between oxides and sulfides because the electrodeposition can achieve a strong adsorption between the two phases by electrostatic adsorption as well as electrochemical reactions.
Therefore, in this study, to combine the above two positive effects, i.e., amorphization and combination with sulfides, we demonstrate the synthesis of amorphous cobalt oxide layers by forming a VS2 layer on a carbon paper (CP) beforehand. Unlike the flat surface of the CP, the layered structure of VS2 hindered the crystallization of the Co oxides. As a result, amorphous cobalt oxides were deposited on the CP with VS2, denoted as CoOx/VS2/CP. CoOx/VS2/CP exhibited an enhanced catalytic activity and better stability for OER than that of Co3O4/CP. The mechanism of the enhancement is discussed in detail.
NO−3 + H2O + 2e− → NO−2 + 2OH−, | (1) |
Co2+ + 2OH− → Co(OH)2 | (2) |
The redox potential of reaction 1 is calculated to be 0.82 − 0.05916 pH (0.47 V vs. standard hydrogen electrode (SHE) at pH = 6).21 Fig. 1b shows the cyclic voltammogram measured using the CP as the working electrode in a 0.2 M Co(NO3)2 aqueous solution (pH ∼6). The NO3− reduction reaction contributed to the cathodic current. Based on the cyclic voltammogram, −0.7 V vs. Ag/AgCl (saturated KCl) with a relatively small current was chosen to achieve a steady deposition rate. The reason is that a smaller current is related to a slower deposition rate in the electrodeposition, which is beneficial to the growth of crystal nuclei instead of the formation of nucleation process and is also preferable in chrono coulometry because it is easier to control the electronic quantity precisely by a manual method. Fig. 1c shows a chronocoulogram obtained during electrodeposition (see the related chronoamperogram in Fig. S1†). The deposition amount can be controlled by controlling the transferred electric quantity. In this study, the Co deposition amount was distinguished from the electric quantity transferred during electrodeposition. For example, Co3O4/CP (0.1C) indicates that electrons with a charge of 0.1C were transferred during the electrodeposition.
The crystal structure of the cobalt oxides deposited on the CP was characterized by XRD, as shown in Fig. 2a and b. The peaks of the deposited cobalt oxides correspond to the peaks of the reported crystalline Co3O4 (ISCD#36256, see 311 at 16.8°).22 Notably, there are several peaks attributed to the CP. According to Table S1,† the full width at half maximum (FWHM) of the peak at 16.8° decreased (i.e., the crystallinity of the deposited Co3O4 increased) with the increase in the electrodeposition amount, sintering temperature, and time. Fig. 2c and d show SEM images of the CP before and after the electrodeposition of cobalt oxides. In Fig. 2d, mesh structure was formed on the surface of the carbon paper. Compared with the structure of the carbon paper, it can be confirmed that these structures are deposited cobalt oxides with the particle size at about 2 μm. The EDS elemental mapping of cobalt and oxygen in Fig. 2e and f and EDS spectrum in Fig. 2g also suggest the existence of cobalt oxides, which indicates a homogeneous deposition.
The as-deposited Co3O4/CP was directly used as an anode in a water electrolysis system without additional modifications. Fig. 3a shows linear sweep voltammograms obtained by averaging the cyclic voltammograms measured for the Co3O4/CP samples with different Co deposition amounts in an O2-saturated 0.1 M KOH aqueous solution to cancel out the capacitive current. Co3O4/CP used for the OER evaluation was synthesized by annealing at 300 °C for 3 h; only the amount of deposited Co was different. The current densities at 1.6 and 1.7 V vs. RHE (dashed lines in Fig. 3a) increase with the increase in the electrodeposition amount of Co3O4. To investigate this effect, EIS was carried out for all samples at 1.6 V vs. RHE. Nyquist plots of the obtained EIS spectra are presented in Fig. 3b. For the semicircle in high frequency range, charge transferring is the main factor that affects the impedance. After the modification of the carbon paper for all the samples, the size of this semicircle did not change so much. Therefore, the semicircles in the high-frequency range resulted from the charge transfer process between the carbon paper and the electrolyte. The other semicircles in the low-frequency range came from the adsorption/desorption process of OER intermediates.23 Curve fitting was carried out with the equivalent circuit shown in Fig. S2; † the fitted parameters are listed in Table S2.† The system resistance R1 did not change significantly among the samples. The charge transfer resistance R2 and double-layer capacitance C2 did not significantly change among the samples. The close values of double layer capacitance indicate that all the samples have similar electrochemical surface area, which excludes the influence of surface area difference on OER activity. R3 and Q3 are related to the impedance in the adsorption/desorption process of OER intermediates on the catalyst surface. The value change is correlated with the increase in the electrodeposition amount of Co3O4. Therefore, the enhancement in OER activity is mainly associated with the increase in the diffusion rate of the reactants, which is likely caused by the increased number of active sites with a larger deposition amount. Fig. 3c and d show the current densities of the Co3O4/CP samples with different Co deposition amounts at 1.6 and 1.7 V vs. RHE, respectively. The current densities of all samples similarly decreased after 100 cycles, which indicate similar stabilities.
To further increase the catalytic activity and stability of cobalt oxides, VS2 was grown beforehand on the CP to change the morphology and crystallinity of the cobalt oxides. Fig. 4a shows XRD patterns of the synthesized samples, denoted as CoOx/VS2/CP. Notably, no considerable peaks corresponding to VS2 and Co3O4 are observed in the XRD patterns of CoOx/VS2/CP (2C) in Fig. 4a and CoOx/VS2/CP (8C) in Fig. S3,† although the EDS elemental mapping indicates the existence of V, S, and Co. This is contrary to the pattern of Co3O4/CP (2C), where the peaks for Co3O4 were observed. Therefore, the absence of cobalt oxide peaks was not attributed to the deposition of cobalt oxides, but to the existence of VS2. As shown in Fig. 4b, CoOx/VS2/CP (0.5C) exhibits a layer morphology of VS2 even though Co is evenly distributed on the surface, as shown in Fig. 4d (see gradual morphology in CoOx/VS2/CP with Co deposition amount increase in Fig. S4†). The SEM image of VS2 on carbon paper is also displayed in Fig. S4.† The bulks of VS2 with a diameter of about 5 μm can be observed. In each bulk, there exists the characteristic layered structure of VS2. Thus, it is possible that the cobalt hydroxide precursor was deposited by electrodeposition between the layers of VS2. In other words, the VS2 layers hinder the generation of large bulk cobalt oxides, resulting in amorphous cobalt oxides after sintering. In addition, the peaks of VS2 disappeared, although V and S were detected by EDS mapping (Fig. 4d and e) and EDS spectra in Fig. 4f and g. The slight increase in the background of the XRD pattern for CoOx/VS2/CP (2C) indicates the formation of amorphous phases, as shown in Fig. S5.† The XPS spectra in Fig. S6† also suggest that VS2 and cobalt oxides reacted (further evidence is shown in Fig. 5b).
The OER catalytic activity of CoOx/VS2/CP was evaluated by cyclic voltammetry and EIS, as shown in Fig. 5. Before OER measurements, pre-scanning at 1.23–1.83 V vs. RHE at 10 mV s−1 for 20 cycles was carried out to reach a steady state. The anodic and cathodic sweeps of the cyclic voltammograms were averaged to eliminate the influence of the double-layer capacitance. As shown in Fig. 5a, the current density of CoOx/VS2/CP (0.5C) is considerably higher than those of the other samples. Notably, at the potential range of 1.2 to 1.4 V vs. RHE, the current density of CoOx/VS2/CP (0.5C) is too high to be neglected, which should not be attributed to the currents of the OER because the OER does not occur below 1.23 V vs. RHE. To investigate this phenomenon, the linear sweep voltammogram of CoOx/VS2/CP (0.5C) at the 100th cycle is also presented in Fig. 5a (red dashed line). The high current density in the low potential range of 1.2 to 1.43 V vs. RHE decreased to almost 0 after 100 cycles, which indicates that the oxidation reaction is irreversible. The cyclic voltammograms and Nyquist plot of EIS spectra at 100th cycle of VS2 are displayed in Fig. S8.† Compared to the considerable current density in 1st cycle, the current density in 100th cycle in the potential range of 1.2 to 1.5 V shows an obvious decrease, which is due to the irreversible oxidation of S2− ions. However, the oxidation current density of VS2/C is small and cannot reach the high current density of CoOx/VS2/CP (0.5C) from 1.2 to 1.5 V in Fig. 5a. Therefore, the high current density of CoOx/VS2/CP (0.5C) from 1.2 to 1.5 V was attributed mainly to the Co oxidation in CoOx, but not to S2− oxidation in VS2. This was also confirmed by XPS, as shown in Fig. 5b (see the deconvoluted XPS spectra in the Co 2p3/2 region in Fig. S7†).24,25 Before the cyclic voltammetry, Co0, Co2+, and Co3+ existed in CoOx/VS2/CP (0.5C). It is possible that Co0 was generated by the reduction of cobalt oxides or hydroxides with S2− ions during the sintering. After the 100 voltammetry cycles, the ratio of Co0 decreased, while that of Co3+ ions increased, which indicates that the Co oxidation contributes largely to the current at a low OER potential. The comparison of the voltammograms of CoOx/VS2/CP (0.5C) after 100 cycles and Co3O4/CP (0.5C) in the first cycle shows that CoOx/VS2/CP (0.5C) containing the amorphous CoOx exhibited a higher catalytic activity than that of Co3O4/CP (0.5C) containing the crystalized Co3O4.
The Nyquist plots of the EIS spectra at 1.6 V vs. RHE in Fig. 5c show that all samples exhibit similar behaviors in the higher frequency range. However, the behavior in the lower frequency range is quite different. CoOx/VS2/CP (0.5C) exhibits the smallest semicircle among all samples, which indicates fastest diffusion. To make a comparison, the Nyquist plot of CoOx/VS2/CP (0.5C) at the 100th cycle are also displayed in Fig. S9.† Compared to the 1st cycle, the semicircle in the low frequency is smaller, indicating a faster adsorption/desorption process. Furthermore, curve fitting was carried out for Nyquist plots in Fig. 5c using the equivalent circuit in Fig. S2; † the results are listed in Table S3.†R1, R2, and C2 did not change significantly for all samples in Fig. 5c, but the adsorption resistance R3 decreased to a large extent for CoOx/VS2/CP (0.5C) compared to those of the other samples. The smallest R3 and largest Q3 of CoOx/VS2/CP (0.5C) indicate the fastest adsorption/desorption process and the most reaction sites on the catalyst surface, respectively.
Fig. 5d shows the current densities of the CoOx/VS2/CP samples with different Co amounts at 1.7 V in the first cycle and 100th cycle. The currents are well retained after 100 cycles, compared to the currents of Co3O4/CP shown in Fig. 3d. This indicates that the amorphous cobalt oxides deposited on VS2/CP exhibit a better stability in the OER catalysis, likely because the amorphous material does not have grain boundaries that can react or easily dissolve.
By comparing the data in Fig. 3d and 5d, we can see that the electrodeposition time of cobalt has a positive-related effect on the OER activity of Co3O4/CP, but barely affects the OER activity of CoOx/VS2/CP. For Co3O4/CP, the deposited cobalt oxides are crystalized Co3O4 structure, which was confirmed by XRD patterns. With the electron quantity in the electrochemical deposition increase, the amount of Co3O4 increases. Co3O4 plays as the active species in the OER catalysis. Therefore, the amount of Co3O4 increase indicates an increase of the active species, which will result in an obvious increase of current density for OER. For CoOx/VS2/CP, the deposited cobalt oxides are amorphous, where Co exists as Co0, Co2+, and Co3+ at the same time from XPS analysis. The increase in deposition time is not directly related to the active species in OER. Increasing deposition time can also increase the number of cobalt oxides, but the deposition time and active species are not directly related. Thus, an increase in current density can be observed by increasing the deposition time for CoOx/VS2/CP, but it is not as obvious as that for Co3O4/CP.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d2ra00492e |
This journal is © The Royal Society of Chemistry 2022 |