Sayantani Paula,
Bibaswan Sena,
Nirman Chakrabortyb,
Sangita Dasa,
Swastik Mondalb,
Asoke P. Chattopadhyaya and
Sk Imran Ali*a
aDepartment of Chemistry, University of Kalyani, Nadia, West Bengal, India. E-mail: skimranchem18@klyuniv.ac.in
bCSIR-Central Glass and Ceramic Research Institute, Jadavpur, Kolkata, West Bengal, India
First published on 15th March 2022
A pH-regulated hydrothermal synthesis method was employed to synthesize Sb4O5Br2 and Sb4O5Cl2 crystallites. Characterization is done by single crystal X-ray diffraction, powder X-ray diffraction, infra-red spectroscopy, scanning electron microscopy and DFT studies. The compounds crystallize in monoclinic symmetry with a P21/c space group. Complete structural analysis of the Sb4O5Br2 compound by using single crystal X-ray diffraction data is performed for the first time and a comparative study with Sb4O5Cl2 is also discussed. The SEM study reveals that the surface morphology changes with the variation of pH for bromide compounds, whereas pH change does not affect the morphology of the chloride analogues. Electronic band structures of the synthesized oxyhalides were investigated in order to understand their catalytic effects in the dye degradation reactions in dark as well as sunlight conditions.
Efficiency of catalytic activities can be controlled by modifying the morphologies of catalyst-particles and by tuning light absorption abilities and band gaps of catalysts.1,4–10 The change of reaction conditions, e.g., pH regulated synthesis, plays an important role for designing these kinds of catalyst materials depending on the reaction conditions they may form different kinds of phases, sizes, shapes and surfaces.11 As far as light absorption is concerned, much of the solar radiation can be harvested by narrowing the band gap of catalysts to allow the valence electron to be excited by lower energy photons. A photocatalytic reaction can be defined as a chemical reaction in which photons interact with a semiconducting material known as a photocatalyst and facilitate the reaction.12 Plenty of metal oxides (e.g., TiO2, ZnO, MnO2, CeO2, CdO etc.), metal halide perovskites (MHP) (e.g., CsPbX3 (X = I, Br, Cl)) and polymers have been established as photocatalysts so far.13 Recently, oxyhalide and metal oxyhalide compounds have been shown as potential photocatalysts, e.g., Bi2MO4Cl (M = Y/La/Bi), PbBiO2X, Bi12O17Cl2, Bi3O4Cl, Bi24O31ClxBr10−x, PbBiO2Br/BiOBr, PbBiO2Br/UiO-66-NH2 (mpg-C3N4/PbBiO2Br), Bi4NbO8Cl, Bi24O31Cl10.1,2,5,14–16
Visible light responsive photocatalysis is responsible for the photocatalyzed decolorization of a dye in solution via a photoexcitation process.17 Despite substantial research endeavours in the field of visible light responsive photocatalysts during past few decades, development of such materials still remains a challenge for us. It is promising to see that a number of novel catalysts have been reported, such as Ce(IO3)4, CeGeO4, ZrHIO6·4H2O, CeHIO6·4H2O, Fe2O3–CeO2–TiO2/γ-Al2O3, Ce-doped MoO3, CuO–MoO3–P2O5, ZnO/MoO3/SiO2, Pt–HCa2Nb3O10, ZrGeO4, which have the ability to degrade organic dyes in the dark condition even at room temperature.18–28
Oxyhalides comprising p-block elements are classified as the members of the [L–O–X] family (L = p-element lone-pair cation, X = halide ion). Some well-known oxyhalides with group 15 cations (Sb3+, Bi3+), that have been reported to date are SbOCl,29 onoratoite,30 Sb3O4Cl,31 Sb4O5Cl2,32,33 Sb8O11Cl2,34 Bi3O4Br, BiOBr.35 Presence of both the halide ions and the electronic lone pair of the cations generate an interesting stereochemical environment in the oxyhalide (X = Cl/Br) compounds. They introduce a special channel or void space or a layered zone inside the crystal structures, where both the units are bound by weak van der Waals interactions.35 In these materials, chlorine and bromine are located between layers, formed by L cations and O anions.
In this work, we have prepared single crystals of both Sb4O5Br2 and Sb4O5Cl2 by hydrothermal technique. A series of both compounds were prepared by varying the pH level using the hydrothermal method. Structural studies of Sb4O5Br2 were previously performed by Maja Edstrand and coworkers by using ‘Patterson project’ in 1947, but the authors did not specify the nature of the antimony bonds and uncertainties associated with the positions of the oxygen atoms.32 In our study, for the first time, we have eliminated these disadvantages and presented a comprehensive structural analysis of compound Sb4O5Br2 using single-crystal X-ray diffraction data and a comparative study with Sb4O5Cl2 has also been discussed. Dye degradation reactions using both Sb4O5Br2 and Sb4O5Cl2 catalyst under both dark and sunlight conditions have also been investigated for the first time and a comparative study of the electronic band energies of the synthesized catalysts is also shown.
A powder X-ray diffraction study was used to determine the phase purity of the prepared compounds, and the raw data were obtained using a Panalytical X'Pert PRO X-ray powder diffractometer in Bragg Brentano geometry with Cu Kα radiation (=1.54060 Å). A fast scanning mode was implemented in 2θ, which ranged from 4° to 70° with a step size of 0.0131°. Each observed reflection was indexed on the basis of the refined crystal structure obtained from the single-crystal data. The powder diffraction pattern was checked and refined using JANA 2006 and the data is well matched with the single-crystal structure refinement data (see Fig. S2 and S3†).
FTIR spectroscopic studies were carried out using a PerkinElmer L 120-000A spectrometer in the region of 4000–400 cm−1. Density Functional Theoretic (DFT) studies were carried out on the crystal structures of the two compounds with the LANL2DZ basis set40,41 and PBE density functional42 using the Gaussian 09W program suite.43 The vibration frequencies were calculated. These were fitted with a FORTRAN program and theoretical FTIR plots were generated.
Morphological characterization of the samples was performed by means of Field Emission Scanning Electron Microscope (FESEM), Zigma, Carl Zeiss, Germany, 30 kV, image resolution: 1.3 nm, energy resolution ∼127 eV. Powder samples have been dispersed in IPA medium (for 30 minutes) and dropped on a glass substrate, followed by drying under an IR lamp for SEM study.
Standard methyl orange (MO) was used for the dye degradation reactions, which were performed in both the absence and presence of sunlight. The synthesized catalysts were dissolved into the MO solution (10 ppm). The solution was stirred in the absence of light for hours until it reached adsorption equilibrium. Then they were irradiated by sunlight (UV irradiation source) with continuous stirring. During that time, solutions were collected and measured at 30 minutes intervals until degradation was completed. The decolorization reaction of catalyzed MO solution in both dark and light conditions was then monitored by a UV-Vis spectrophotometer. The optimal value for taking the amount of catalyst and the dye concentration was chosen after several experiments.
The catalysts were also dissolved in aqueous solution to compare the spectra against the MO-dye solution. The absorbance spectra of both the aqueous and dye solutions of each catalyst were studied by the spectrophotometer by changing the wavelength from 200 nm to 900 nm, from which λmax values were obtained in each case. The absorbance values were measured for each solution at fixed λmax value for each case obtained previously. The reaction was started at room temperature and after complete degradation in presence of sunlight, the temperature turned to around 35 °C.
Chemical formula | Sb4O5Br2 | Sb4O5Cl2 | Sb4O5Cl2 (ref. 33) |
---|---|---|---|
Formula weight/g mol−1 | 726.82 | 637.90 | 637.90 |
Temperature/K | 293 | 293 | — |
Crystal system | Monoclinic | Monoclinic | Monoclinic |
Space group | P21/c (14) | P21/c (14) | P21/c (14) |
a/Å | 6.6073(10) | 6.2435(3) | 6.2393(8) |
b/Å | 5.1428(10) | 5.11440(10) | 5.1132(7) |
c/Å | 13.4696(2) | 13.5502(6) | 13.5351(18) |
β/deg | 97.9328(11) | 97.252(3) | 97.14(2) |
V/Å3 | 453.317(13) | 429.22(3) | 428.43(10) |
ρ/g cm−3 | 5.3247 | 4.9357 | 4.495 |
Z | 2 | 2 | 2 |
Wavelength/Å | 0.71073 | 0.71073 | — |
Indices range | −14 ≤ h ≤ 13 | −12 ≤ h ≤ 12 | — |
−10 ≤ k ≤ 10 | −10 ≤ k ≤ 10 | ||
−28 ≤ l ≤ 28 | −26 ≤ l ≤ 26 | ||
No. of reflections measured/unique | 35836/4611 | 35050/3541 | 2293/929 |
Rint | 2.42 | 3.41 | — |
(sinθ/λ)max/Å−1 | 0.8 | 0.8 | — |
R(obs)/wR(all) | 2.42/2.91 | 3.24/3.63 | 5.38/1.47 |
Δρmax/Δρmin | 0.70/−0.68 | 3.22/−1.45 | — |
GOF(obs)/GOF(all) | 1.49/1.41 | 1.44/1.28 | — |
Table 2 summarizes all Sb–O distances found in [(Sb4O5)2+]n units. The Br− ions are located between the [(Sb4O5)2+]n layers. There is no direct covalent bond between antimony and the halide atom (Br1) as the bond length is more than 3 Å, whereas, the normal covalent bond length of Sb–Br is in the range of 2.46–2.54 Å.44 A comprehensive structural analysis has been performed in this study and repaired the uncertainties over the atomic positions mentioned by Maja Edstrand in 1947.32
Atoms | Oxygens | Distance (Å) |
---|---|---|
Sb1 | O1 | 1.963(3) |
O1 | 2.059(3) | |
O3 | 2.011(3) | |
Sb2 | O1 | 2.460(3) |
O2 | 1.8997(2) | |
O3 | 2.079(2) | |
O3 | 2.145(2) |
The study also shows more precise structural parameters of Sb4O5Cl2 than the previously reported antimony oxychloride compound (see Table 1).32,33 The lower R value for the model obtained from our experiment is also indicative of a better structural model. When Sb4O5Br2 is compared to Sb4O5Cl2, slight elongation along the a and b axes is observed in Sb4O5Br2, whereas slight elongation along the c axis is observed in Sb4O5Cl2. This result is well suited to the larger Sb–Br bond distance (3.004 Å) compared to the Sb–Cl bond distance (2.94 Å), which means the van der Waals gap is higher in between [Sb4O52+] layers in Sb4O5Br2. The lone pairs present in Sb (1) and Sb (2) are directed away from the layer. Corresponding Sb–O bond lengths for antimony oxy-chloride are listed in Table 3. The Sb–O distances are found to be comparable with the distances found in cubic Sb2O3 and orthorhombic Sb2O3.45
Atoms | Oxygens | Distance (Å) |
---|---|---|
Sb1 | O1 | 1.9708(14) |
O1 | 2.0715(16) | |
O3 | 2.0130(14) | |
Sb2 | O1 | 2.4060(15) |
O2 | 1.90154(12) | |
O3 | 2.0688(15) | |
O3 | 2.1690(13) |
The electronic band structures of the synthesized crystallite samples Sb4O5Br2 and Sb4O5Cl2 are obtained in both aqueous and dye solution, were analyzed by UV-Vis absorption spectra and Tauc plots are also shown. In this case, the corresponding λmax was obtained at around 364 nm in the aqueous system for both compounds, but in the dye solution it varied with the change of pH. The absorption spectra of the samples are shown in Fig. 5, 6, 7 and 8 respectively. For the Sb4O5Br2 samples, the λmax values are more red shifted, showing highest λmax for pH = 6 at about 500 nm, while in case of the Sb4O5Cl2, it shows almost similar λmax (∼500 nm) at pH = 2,5,6, whereas at pH = 3 and 4, λmax is obtained at 465 nm and 476 nm, respectivevly.
In a conventional semiconductor, the direct band gap energies can be calculated by the Tauc equation:
(αhν)2 = A(hν − Eg) |
Fig. 13 presents the plot of the concentration (Ct/C0) of MO solution versus the reaction time (t) of Sb4O5Br2 samples prepared at pH = 2, 3, 4, 5, 6 respectively. This degradation process of MO is in accordance with the first-order kinetics model of the Langmuir–Hinshelwood equation, and is expressed as:
ln(C0/Ct) = kt + x, |
The energy gap is very similar for both Sb4O5Br2 and Sb4O5Cl2, which is about 3.4 eV, obtained from the aqueous solutions. It varies largely when the dye solution of MO with synthesized catalysts is used and lowered to about 2.2–2.3 eV for both compounds. This variation may be due to interference from MO dye solution itself, since the values of the absorption coefficient, in this case, are the sum of the spectra of both the MO dye and the Sb4O5X2 compounds. Therefore, it can be concluded that to obtain the accurate band gap values, only aqueous solutions should be used, which can be the characteristic bandgap for the semiconductor itself.46 Yang et al. also studied the band gaps for the Sb4O5Cl2 compound at different pH and the value is about 3.3 eV.11
The band gap values are also well matched with the computational study carried out by Ran et al.47 The band gap energies of Sb4O5Br2 compounds vary from 3.4 eV to 3.47 eV with the change of pH (Fig. 9). A relatively slight smaller band gap has been found at pH = 2 (3.4 eV). These compounds may be promising as solar absorbers in the UV region.11,47
Scanning electron microscopic study reveals that needle shaped particles at pH = 2, 3 transform into hexagonal cluster shaped particles at pH = 5, 6 while both needle and clusters of hexagons are observed at pH = 4. Henceforth, it can be concluded that the surface morphology of the products is transformed well in accordance with the acidity of precursor solutions (Fig. 17 and 18). However, no such morphological changes were observed for Sb4O5Cl2 by changing the pH. The shape and size of the particles of both Sb4O5Br2 and Sb4O5Cl2 have been listed in ESI (Table S4†).
Fig. 17 SEM images of antimony oxybromide at (a) pH = 2, (b) pH = 3, (c) pH = 4, (d) pH = 5, (e) pH = 6. |
Fig. 18 SEM images of antimony oxychloride at (a) pH = 2, (b) pH = 3, (c) pH = 4, (d) pH = 5, (e) pH = 6. |
Yang et al. also reported a slight change in surface morphology due to the change of pH of hydrothermally synthesized Sb4O5Cl2 crystallite (160 °C for 12 h).11 It showed hollow sphere shape with irregular cuboids at pH = 2 and it transforms into microbelt like particles at higher pH.
From the above study, it could be suggested that the compounds with large surface areas effectively adsorb the dye molecules, which leads to the rupture of labile azo bonds of the methyl orange dye and furnishes free electrons that may cause the dye degradation for certain compounds at dark conditions, as those electrons have the capability to form reactive oxygen species (ROS), i.e., superoxide radical anions and hydroxyl radicals.20,48,49 However, due to the absence of conducting metals in the synthesized compounds, only partial dye degradation could be achieved in dark conditions. Furthermore, the solution is subjected to solar light illumination after it attains adsorption–desorption equilibrium, and as a result, ROS get produced again and causes further dye degradation.1,11,50 Although complete degradation is not possible, which could probably due to the formation of some by-products. The probable mechanism of dye degradation in both dark and light condition is proposed as follows:
In dark condition:
Sb4O5X2 + MO → Sb4O5X2 (MO) |
Sb4O5X2 (MO) ↔ Sb4O5X2 + MO+ + e− |
e− + O2 → ˙O2− |
˙O2− + H+ → HO2˙ |
2HO2˙ → H2O2 + O2 |
H2O2 + e− → HO˙ + HO− |
HO˙ + MO/MO+ → … → by-products |
In presence of sunlight:
Sb4O5X2 + hν → Sb4O5X2 (eCB− + hVB+) |
HO− + hVB+ → HO˙ |
H2O + hVB+ → HO˙ + H+ |
eCB− + O2 → ˙O2− |
˙O2− + H+ → HO2˙ |
2HO2˙ → ˙H2O2 + O2 |
H2O2 + e− → HO˙ + HO− |
HO˙ + MO → CO2 + H2O + by-products |
Scanning electron microscopic studies reveal that needle shaped particles transform into hexagonal cluster shaped particles by increasing the pH for Sb4O5Br2, although no such morphological changes were observed for Sb4O5Cl2 by changing the pH. A comparative study to check the dye degradation (MO) using both compounds confirmed that the Sb4O5Br2 samples showed better (approximately 59%) degradation overall (both under dark and light conditions) at pH = 6 and it reduces up to 6% by lowering the pH. However, the Sb4O5Cl2 catalytic dye degradation was less dependent on pH, as it varied from 36% to 45% (both under dark and light conditions) under different acidic conditions, which is well justified to their SEM analysis because of the morphology remained the same upon pH change.
The band gap obtained in aqueous solution using Sb4O5Br2 samples is around ∼3.4 eV, while it varies from 2.2 to 2.37 eV in MO dye solution. Similarly, the energy gaps calculated from aqueous and dye solutions of Sb4O5Cl2 samples are around 3.4 eV and 2.19–2.35 eV, respectively. The electronic band structures, calculated using the aqueous solution of the prepared compounds, reveals wide band gap nature for both synthesized semiconductors. Due to the interference of the dye molecules, the dye mixed aqueous solution of the synthesized catalyst provides lower band gaps than the aqueous solution of the dye-free synthesized catalyst. Therefore, the accurate band gap values can be estimated only from the aqueous solutions of the catalyst, which can be considered as the characteristic bandgap of the semiconductor itself.
Footnote |
† Electronic supplementary information (ESI) available. CCDC 2119417 and 2119418. For ESI and crystallographic data in CIF or other electronic format see DOI: 10.1039/d2ra01215d |
This journal is © The Royal Society of Chemistry 2022 |