Sujit Bhand,
Plawan Kumar Jha and
Nirmalya Ballav*
Department of Chemistry, Indian Institute of Science Education and Research (IISER), Dr Homi Bhabha Road, Pune, 411 008, India. E-mail: nballav@iiserpune.ac.in
First published on 20th October 2022
Reduced graphene oxide (rGO) has emerged as an excellent interfacial material for improvising the performance of dye-sensitized solar cells (DSSC). Herein, we have applied rGO as interfacial layers between a fluorine doped tin oxide (FTO) coated glass substrate and semiconducting material TiO2 in a photoanode of a DSSC which showed an unusual enhancement in generating a photocurrent in comparison to the control (without rGO layers). An electrochemical impedance spectroscopy (EIS) study was performed to gain the mechanistic insights into such a remarkable enhancement of photoelectric conversion efficiency (PCE) which revealed improved charge transfer and suppressed charge recombination due to high-electrical conductivity and probably more negative work function of our rGO material compared to the bare TiO2 photoanode.
The interface associated with transparent conducting glass such as fluorine-doped tin oxide (FTO) and TiO2 is extremely important as it creates a conducting path for the electrons in the device. Also, at this location, the possibility of electron–hole recombination is very high which ultimately hampers the performance of the DSSC. Fig. 1 presents the schematic representation of a DSSC device depicting various interfaces and charge movement. Applying various nanomaterials, such as, graphene,10–14 carbon nanotubes (CNT)13,14 and gold/platinum nanoparticles15 in a photoanode could reduce the rate of charge recombination, therefore, improved the PCE of DSSCs.16 Out of which, graphene-based materials possessing excellent physicochemical properties have emerged as promising candidates for the enhancement of the efficiency of DSSC. In the combination of TiO2 and functionalized graphene materials, such as, reduced graphene oxide (rGO), the electron transfer rate increases at the interface.17 However, blending micron size rGO nanosheets along with nanosized (<25 nm) porous TiO2 could introduce more grain boundaries in the layer which in turn could obstruct the charge flow and underestimate the efficiency of DSSC.18 In the context of such interface engineering in DSSC with rGO an inevitable question is: how important is the quality of rGO? Also, there are numerous investigations on DSSC,19,20 whereby the FTO surface was decorated with a compact thin layer of TiO2 made from TiCl4; however, such films are air and moisture sensitive and can degrade over time, therefore ambient stability is an unavoidable issue.
Herein, we have modified the FTO/TiO2 interface by self-healed rGO generated from rather unconventional wet-chemical reduction methods. Specifically, rGOs with distinctive two-dimensional (2D) and three-dimensional (3D) morphological patterns, rGO1 (GO to rGO reduction was done with the Fe(II) salt)21 and rGO2 (GO to rGO reduction was done with the Cu(I) salt),22 respectively, were explored. A schematic view of our DSSC involving interfacial rGO layers along with FESEM images of rGO1 and rGO2 is presented in Fig. 1. The interfacial layers of rGO on the FTO can behave as an extended electron collecting electrode, as successfully demonstrated by Chen et al.,17 eventually improving the electron-transport rate in DSSC. As a result, the PCE values of our DSSC devices fabricated at ambient conditions were realized to be noticeably higher than previous reports which is the primary highlight of the present study. An easy comparison of the present work over earlier literature can be assessed from Table S1.†
D1: bare FTO coated glass was used as the current collector. D2: FTO coated glass was kept in the 50 mM aqueous solution of TiCl4 at 70 °C for 15 min followed by 30 min heating at 125 °C. D3: ∼1 mg/1.5 mL dispersion of rGO1 (30 min sonication in N-methylpyrrolidone (NMP) was coated on FTO coated glass by spin coating method (800 rpm s−1; 60 s) and dried by heating at 200 °C for 10 min. D4: similar as D3 just rGO2 was used instead of rGO1. About 7–10 μm thick transparent TiO2 was doctor-bladed over treated FTO substrate, kept steady at room temperature for 10 min, and heated at 125 °C for 15 s. After that 16 μm thick layer of opaque TiO2 paste was coated using the doctor-blade method, kept for 5 min at room temperature, then sintered at 350 °C for 15 min, 450 °C for 30 min and 500 °C for 30 min. For the dye absorption, photoelectrodes were immersed in 0.3 mM N719 dye (in ethanol) for 3 h at room temperature followed by thorough rinsing with ethanol to remove excess dye and dried in air. For the device assembly, photoanode and conductive platinised-glass counter electrode (with hole diameter of 0.75 mm) were sandwiched and sealed with 60 μm thermoplastic Surlyn spacer at 100 °C for 10 s. The commercial iodine-based liquid electrolyte was introduced into the sandwich cells through holes in the counter electrode. Please note that, the PCE values shown in Table 1 is the average of 10 devices and the % PCE of all fabricated devices are presented in Fig. S5.† To estimate loading of dye, photoanode was kept in 10 mL ethanol and aqueous NaOH (1 M) solution and absorption spectra recorded.12
The FESEM images showed micron-sized and well-distributed rGO1 and rGO2 on the rGO treated FTO, without any significant change in surface morphologies, though, heated at high-temperature (Fig. S1†). Characteristic signatures of the D and G band in the Raman spectra is evidenced of the fact that rGO backbones were primarily retained even after the heat treatment (Fig. S2a†). The coating of TiO2 (both transparent and opaque mesoporous layers) was observed to be around 23 μm thick without any cracking and peeling even after annealing at ∼500 °C (Fig. S3 and S4†). The light transmission properties of the FTO in all the devices were evaluated by the solid-state UV-vis spectroscopy (Fig. S2b†). About 84% transmittance was observed for bare the FTO (D1). Interestingly, the transparency was almost maintained after successful integration of the interfacial layers of rGOs (∼82–83%) which suggests that the photosensitizer dye in DSSC devices could be well-illuminated without severe photon loss during the measurements. Solid-state absorption spectra of dye decorated photoanode revealed characteristic electronic transition signatures of N719 (Fig. S6†).
Performance of the DSSC devices D1, D2, D3 and D4 were realised under 1 sun illumination. The short circuit current density (JSC), open circuit voltage (Voc), fill factor (FF), and power conversion efficiency (PCE) for D1 was found to be around 14.88 mA cm−2, 0.7 V, 0.57, and 6.08% respectively (Table 1 and Fig. 2b). Interestingly, after the rGO modification (D3) the JSC increased dramatically to 17.89 mA cm−2, resulting in the PCE value of 8.08%.
D1 | D2 | D3 | D4 | |
---|---|---|---|---|
Blank | TiCl4 | rGO1 | rGO2 | |
JSC (mA cm−2) | 14.88 | 15.65 | 17.89 | 17.91 |
Voc (V) | 0.70 | 0.67 | 0.66 | 0.66 |
Fill factor (FF) | 0.57 | 0.64 | 0.67 | 0.67 |
% efficiency | 6.08 ± 0.5 | 6.80 ± 0.5 | 8.08 ± 0.2 | 8.01 ± 0.3 |
Such an enhancement clearly evidenced an alteration of the interfacial energy alignment upon incorporation of the rGO even with distinctive morphological patterns. As our synthesized rGO (rGO1) is defect-healed so a higher number of generated electrons at the upper layer (dye) could be easily facilitated towards FTO. Also, due to the distinct work function value of rGO and TiO2 the electron is unable to travel back towards TiO2 leading to higher electron generation as realized from the values of JSC. Although reported rGOs were made by conventional reducing agents, the PCE value of the graphene modified DSSCs is comparable or lower than here reported results (Table S1†) which validates the importance of use of reduced graphene oxide and method of applying rGO on surface instead of using it in TiO2 paste. On the other hand, the PCE of D2 and D4 found to be 6.80 and 8.01% respectively emphasizing the significance of rGO at the interfaces of TiO2/FTO.
Considering the fact that the minute changes in interfacial resistance greatly alter the DSSCs performance, electrochemical impedance spectroscopy (EIS) measurements were performed. Upon fitting the Nyquist plots by the equivalent circuit (as shown in Fig. 3), two semicircles appeared that can be assigned as resistance 1 (R1, first) and resistance 2 (R2, second). The intercept at real Z-axis is the equivalent series resistance (Rs) showing the total resistance created by the internal components of DSSC. Rs of the D3 and D4 was found to be ∼30.4 and 34.0 Ω, respectively, which is slightly higher than control devices (D1 and D2) (Table 2). Also, the Rs of D3 was found to be lower than D4 which could be due to the higher electrical conductivity of rGO1 (500 S m−1)21 compared to rGO2 (150 S m−1)22 ultimately affecting the JSC and PCE.
Fig. 3 Typical Nyquist plots obtained from the DSSC devices D1, D2, D3 and D4. Experimental data points were fitted with an equivalent circuit schematically shown in the inset. |
Device | Rs [Ω] | R2 [Ω] | ωmax [Hz] | τe |
---|---|---|---|---|
D1 | 22.8 | 10.2 | 52 | 3.06 |
D2 | 29.1 | 7.5 | 48 | 3.31 |
D3 | 30.4 | 10.4 | 45 | 3.54 |
D4 | 34.0 | 9.1 | 46 | 3.46 |
The interface between electrolyte and counter electrode was unaltered for all the devices therefore R1 (2.1, 1.2, 1.7, 2.1 Ω for D1, D2, D3, D4, respectively) was realised to be similar except for D2 where TiO2 layer prepared by chemical method acted as a blocking layer. R2 is the resistance created at the electrolyte/dye/TiO2 interface which is found to be 10.2, 7.5, 10.4, and 9.1 Ω for devices D1, D2, D3, and D4, respectively. The lowest R2 value of D2 is because TiO2 prepared from specific concentration23 of TiCl4.
The electron lifetime (τe) can be expressed as τe = 1/(2πωmax) where ωmax is the maximum frequency calculated from the semicircle. For D1 and D2 the τe values were found to be around 3.06 and 3.31 ms, respectively, however, after the rGO coating, the τe of device D3 and D4 increased to 3.54 and 3.46 ms, respectively, which clearly endorsing the importance of rGO on the reduction of charge-recombination process24 in DSSC. Furthermore, the absorption spectra of dye de-absorption solution from photoanode revealed that the dye loading was almost similar across the devices (Fig. S7†). Overall, it can be concluded that mere spin coating of rGO at the TiO2/FTO interface is good enough for enhancing the performance of DSSC devices.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ra05375f |
This journal is © The Royal Society of Chemistry 2022 |