Mohsen Rostami Sakhaa,
Parya Halimitabriziab,
Saeed Soltanali*c,
Fatemeh Ektefac,
Zeinab Hajjard and
Dariush Salaria
aReactor and Catalysis Research Lab., Department of Chemistry, University of Tabriz, Iran
bDepartment of Chemical and Petroleum Engineering, University of Tabriz, Iran
cCatalysis Technologies Development Division, Research Institute of Petroleum Industry (RIPI), Tehran, Iran. E-mail: soltanalis@ripi.ir; sssoltan@gmail.com
dNanotechnology Research Division, Research Institute of Petroleum Industry (RIPI), Tehran, Iran
First published on 8th March 2023
Investigation of the current industrial processes, such as methanol to olefin (MTO) and hexane to olefin (HTO), in terms of green and sustainable chemistry approaches in order to design the process, catalyst and reactor from the beginning in such a way as to minimize environmental pollution is compulsory. Therefore, the synthesis of a group of multifunctional catalysts, which can be used simultaneously in both industrial processes to produce a variety of products, was studied. The effect of incorporation of different metals (Fe, Mn, Zn, Ga and Al) on the strengthening of each of the products was also studied. The investigation of reactor productivity (WHSVHTO = 25) in HTO showed that the production efficiency of propylene in microchannels is higher than the ideal value for all samples, which is a significant improvement for sustainable approaches in future technologies. Considering the overall performances, Ga-ZM showed the best performance in both processes due to the high P/E ratio. The significant effect of Ga on the increasing of propylene was confirmed in MTO at 400 °C (P/E ≃ ∞), which indicated the dramatic effect of this metal in directing the reaction mechanism to an olefin-based cycle by converting almost all ethylene to propylene by methylation.
By synthesizing catalysts, which can perform optimally in several reactions (multifunctional catalysts) and performing the processes under milder conditions by modern technologies, propylene can be produced by both MTO and naphtha cracking processes through a sustainable approach.15 Zeolites with different topologies, acidic properties and morphologies facilitate the production of desirable products based on the type of reactants and the operating conditions in various processes. In fact, the framework of zeolites can be optimized based on the purpose.16–18 Meanwhile, ZSM-5 zeolite with microporous structure is a versatile catalyst with a great impact on catalytic applications due to its shape selectivity. It should be noted that ZSM-5 typically suffers from simple microporous structure, long diffusion paths, and strong additional acid sites, which ultimately leads to low catalytic activity in both MTO and HTO processes.19–21 Improving the proper methods of ZSM-5 synthesis makes it possible to overcome the limitations while maintaining its ability to produce the desired products. In other words, proper synthesis allows the growth of nanoscale crystal structures, hierarchically with different pore types without using additional chemicals.22,23 Simultaneously, the limitations preventing the using of ZSM-5 in both MTO and HTO processes can be minimized by altering the acidic properties.24,25 Changing the pore structure and acidity of ZSM-5 enhances its catalytic activity and selectivity to light olefins, making it a key catalyst in the chemical industry. ZSM-5 catalysts can achieve the goals of green chemistry when the desired structural properties are formed by using environmentally friendly conditions and compound in addition to increasing the production of the desired product.
Generally, catalytic reactions are limited due to the poor heat and mass transfer performance; therefore, the catalyst efficiency and lifetime are minimized. The high surface area-to-volume (SAV) ratio (typically about 10–100 times more than conventional reactors) in microchannel reactors enhance the catalyst efficiency in comparison with fixed- and fluidized-bed reactors. The correction of temperature fluctuations in microchannels, which prevents the formation of hot spots along the catalytic bed during exothermic processes as well as enhancing the proper conduction of heat along the catalytic bed during the endothermic processes, is immediately possible. Microchannel technology is a modern approach, which minimizes the negative environmental impacts on a wide range of chemical products. According to the principles of green chemistry, microchannels can play an essential role in achieving sustainable catalytic processes.26–31
In the present study, for the first time, sustainable chemistry approaches based on the metrics recently proposed by Shell have been given first priority. Therefore, the feed flow was increased compared to the two recent reports by this group to investigate the effect of various incorporated metals in MTO and HTO processes, using microchannels. Additionally, the effect of temperature was studied in MTO to reduce energy consumption in the performance of incorporated zeolites. The synthesized zeolites were obtained under milder conditions (less template consumption, lower crystallization temperature, using non-templating method to achieve hierarchical zeolites, and less crystallization time) compared to our previous works in order to obtain cleaner products in terms of green and sustainable chemistry. Furthermore, the effect of metal substitution on the textural and acidic properties as well as the performance in two industrial processes in order to achieve multifunctional catalysts was studied.
RH = required hours of stability to decrease the catalyst consumption to the ideal value.
The SEM images (Fig. 2) of the incorporated zeolites illustrated the formation of uniform nanocrystals (<100 nm) due to optimal synthesis conditions and fluoride environment. In addition, all zeolites, except Zn-ZM, demonstrated almost the same particle size due to the low amounts of substituted metals. Furthermore, the lack of extra-structural species was proved by the surface clarity of the formed particles, which was in line with the XRD profiles. The compounds used in the synthesis as well as the operated synthesis method in the preparation of the catalysts, which were incorporated with the various metals, showed no accumulation of elements and a significantly uniform distribution of the elements in the mapping images (Fig. 3), which also confirmed the incorporation of metals into the structure and/or uniform dispersion in the cavities and surfaces of catalysts.31,32
Fig. 4 shows the N2 adsorption–desorption isotherms of BET for the incorporated zeolites. The formation of type IV isotherm was quite evident in the study of the relevant isotherms, which indicated the formation of mesopores in zeolites incorporated with different metals. Mesoporous structures enhance the transfer of products from the catalytic bed and ultimately increase their activity and stability. The obtained pore size distribution profiles (Fig. 5) also showed that all samples had pores in the range of 1–6 nm, which indicated the formation of narrow mesopore structures and super-uniform nanocrystals. All the incorporated catalysts showed a combination of types H2, H3 and H4 hysteresis loops due to a sharp increase of the slope in the range of P/P0 > 0.4, with capillary condensation. This combination indicated the formation of interconnected mesopores, which confirmed the homogeneous nanocrystalline structures in SEM images. In addition, the hysteresis loop in the range of P/P0 > 0.9 indicated the presence of wider and larger mesopores in all samples, which was carefully in line with pore size distribution curves. According to Table 1, high external surface area was also formed in all samples, which is in agreement with the formation of mesoporous structures.33–35
Catalyst | SBETa | Sextb | Sext/SBET | Vtc | Vmicd | Vmese | df |
---|---|---|---|---|---|---|---|
a The specific surface area (m2 g−1).b The external surface area (m2 g−1).c The total pore volume (cm3 g−1).d The micropore volume (cm3 g−1).e The mesopore volume (cm3 g−1).f The average pore diameter (nm). | |||||||
Fe-ZM | 340 | 200 | 0.59 | 0.18 | 0.06 | 0.12 | 2.17 |
Zn-ZM | 385 | 250 | 0.65 | 0.21 | 0.06 | 0.15 | 2.23 |
Al-ZM | 364 | 251 | 0.69 | 0.22 | 0.06 | 0.16 | 2.37 |
Mn-ZM | 340 | 197 | 0.58 | 0.20 | 0.07 | 0.13 | 2.38 |
Ga-ZM | 361 | 220 | 0.61 | 0.19 | 0.05 | 0.14 | 2.10 |
Fig. 6 shows the results of ammonia desorption analysis for the substituted samples. The investigate of NH3-TPD data showed that the incorporation of Mn and Ga metals had no effect on the total number of acid sites. However, the presence of Zn in the structure of the synthesized catalysts caused a slight increase in the number of available sites. This phenomenon was probably due to the reaction of Zn with the structural Al and the enhancement of the formation of internal acid sites and partial extra-structural species. According to Table 2, the decrease of the acid strength in both weak and strong acid sites was observed in all substituted samples with different metals because the peaks of weak and strong acid sites, in the temperature range of 150–250 °C and 375–500 °C, respectively, shifted to lower temperatures. Mn-ZM and Fe-ZM showed a more severe peak displacement in the area corresponding to the weak acid sites, due to the severe attenuation of these active sites, which play the major role in the production of light olefins.
Catalyst | Total acid (mmol g−1 ×10) | Weak acid (mmol g−1 ×10) | Strong acid (mmol g−1 ×10) | TWa (°C) | TSb (°C) | W/S | Si/Mc |
---|---|---|---|---|---|---|---|
a The temperature related to weak acidity zone.b The temperature related to strong acidity zone.c Obtained from ICP-OES. | |||||||
Fe-ZM | 0.41 | 0.29 | 0.12 | 140 | 380 | 2.41 | 385 |
Zn-ZM | 0.70 | 0.54 | 0.16 | 180 | 420 | 3.37 | 379 |
Al-ZM | 0.63 | 0.42 | 0.21 | 197 | 437 | 2.00 | 391 |
Mn-ZM | 0.65 | 0.52 | 0.13 | 133 | 408 | 4.00 | 386 |
Ga-ZM | 0.63 | 0.42 | 0.21 | 188 | 400 | 2.00 | 391 |
H2-TPR analysis (Fig. 7) of Ga-ZM and Fe-ZM showed that the synthetic samples lacked extra-structural species because no indicator peak was observed in the range of iron and gallium oxides. Therefore, in confirming the XRD and SEM results, it can be concluded that almost all metals were incorporated in the tetrahedral structure of synthetic zeolites, which results in minimizing the number of Lewis acid sites.
FT-IR analysis (Fig. 8) was used to identify the structural vibrations, relative intensities of Brønsted and Lewis acid sites, and surface silanol groups of the synthesized samples. FT-IR spectra of incorporated zeolites were taken in the range of 400–4000 cm−1. Characteristic peaks of MFI structure were observed for all catalytic samples. The spectra in the wavelengths of 450, 550, 800, 1080 and 1250 cm−1 express the vibrations of the Si–O and Al–O bonds in the internal quadrilateral units of the SiO4 and AlO4, the vibrations within the networks of dual five-membered rings in the intermittent and repetitive structure of MFI, symmetric tensions of external bonds, the internal asymmetric tensile vibrations of Si–O–Si and Si–O–Al bonds and the vibrations of four branched five-membered rings in MFI structure, respectively. A very weak signal was seen in the range of 3650 to 3800 cm−1 for all samples. This signal indicates the vibrations of the O–H bond in can be assign to the Si–OH–Al groups (Brønsted acid sites, 3600 cm−1), extra-framework Al–OH groups (3660 cm−1), and internal and external silanol sites (3700–3750 cm−1), respectively. Moreover, the low intensity of peak is the confirmation of low amount of Brønsted acid sites in the structure of incorporated zeolites.36–39
UV-vis analysis (Fig. 9) examines the coordination states of zeolites which indicates whether oxidation of metal ions is located in zeolite structure or not? UV-visible analysis of Fe-ZM sample showed the absorption range of 190 to 1100 nm. The specific peak of Fe-ZM (230 nm) was seen clearly which is related to the charge transferring from oxygen to Fe and it can be concluded that Fe ions exist in the tetrahedral coordination structure of inner framework of zeolite.40
According to Tables 2 and 3, Al-ZM produced the highest P/E ratio in HTO, which showed that strong and weak acid sites played the most important role in increasing the production of propylene in the catalytic cracking processes. Total olefin yield (TOY) and the selectivity of light olefins in Fe-ZM from the 6th hour of reaction onwards showed a clear decrease, indicating the blockage of some acid sites. In fact, Fe forms moderate acid sites, which enhance the production of propylene but limit the production of other olefins,41,42 as evidenced by the high P/E ratio of Fe-ZM after Al-ZM. The highest TOY was also related to Al-ZM and Ga-ZM samples (Fig. 11). Therefore, to increase the production of propylene in the cracking processes in high WHSV using a green and sustainable catalyst, Al-ZM was introduced, which had the highest P/E ratio and TOY.
Conv. (%) | S(Alkanes) (%) | (%) & (%) | (%) | S(BTX) (%) | TOY (%) | P/E | ||
---|---|---|---|---|---|---|---|---|
HTO | Fe-ZM | 88.8 | 24 | 16.25, 35.75 | 6.2 | 17.8 | 49.6 | 2.2 |
Mn-ZM | 81.8 | 29.3 | 17.76, 35.54 | 12.2 | 5.2 | 53.6 | 2 | |
Zn-ZM | 100 | 18 | 18.74, 31.86 | 3.9 | 27.4 | 54.5 | 1.7 | |
Ga-ZM | 90.5 | 27.8 | 17.96, 37.73 | 10.4 | 6.2 | 59.8 | 2.1 | |
Al-ZM | 87.9 | 30.2 | 14.91, 38.78 | 15.3 | 0.9 | 60.6 | 2.6 | |
MTO (450 °C) | Fe-ZM | 100 | 22.2 | 5.50, 50.1 | 22.6 | <0.1 | 78.2 | 9.1 |
Mn-ZM | 100 | 22.3 | 4.71, 48 | 25.6 | <0.1 | 78.4 | 10.2 | |
Zn-ZM | 100 | 39.2 | 10.5, 33.6 | 13.9 | 4.3 | 58 | 3.2 | |
Ga-ZM | 100 | 16.9 | 9.78, 46.01 | 27.1 | 0.5 | 82.9 | 4.7 | |
Al-ZM | 100 | 20.3 | 13.23, 42.36 | 23.5 | 0.6 | 79.1 | 3.2 | |
MTO (400 °C) | Fe-ZM | 100 | 13 | 4.59, 51.4 | 30.8 | <0.1 | 86.8 | 11.2 |
Mn-ZM | 100 | 15.3 | 4.91, 48.18 | 30.5 | 0.2 | 83.6 | 9.8 | |
Zn-ZM | 100 | 16.2 | 11.59, 42.9 | 25.5 | 3.3 | 80 | 3.7 | |
Ga-ZM | 100 | 14.7 | 0, 50.5 | 33.2 | 0.3 | 83.7 | ∞ | |
Al-ZM | 100 | 18.6 | 11.02, 40.77 | 28.6 | 0.6 | 80.4 | 3.7 |
The investigation of the performance of the samples at 450 °C showed that over time, the selectivity of light olefins and TOY increased, which was the most obvious in Zn-ZM. Considering the performance of this sample in HTO and the presence of minor extra-structural species, this species facilitated the conversion of methanol to olefins over time by strengthening the olefin-based cycle. However, the lower ratio of P/E in comparison with other samples showed that much more ethylene was produced which confirmed the results of HTO. Indeed, the more production of ethylene and arenes is a sign of the dominance arene based cycle in MTO.43–45 Therefore, in the micro-meso-macroporous system, by preventing over reactions in MTO, the production of aromatics (which was significant in HTO) was limited, and instead ethylene was produced. On the other hand, the reduction of temperature in the study of Zn-ZM showed that from the 6th hour onwards, TOY and the selectivity of light olefins decreased, which is a sign of the obstruction of active acid sites in the production of light olefins. Reducing the temperature in the MTO also lead to the strengthening of the arene based cycle, which in general leads to the production of aromatics (as the precursors of coke formation) and ethylene, and thus the beginning of mesoporous occlusion. The dramatic increase of TOY at 400 °C compared to 450 °C (80% vs. 58%) also proved the claim of strengthening the arene based cycle. In fact, lowering the temperature had the highest impact on the increasing of TOY and the selectivity of light olefins. The high production of alkanes in Zn-ZM seemed to be due to the presence of Lewis acid sites, which convert more ethylenic and aromatic intermediates to alkanes by enhancing the elimination of hydrogen from the system. The decreasing of reaction temperature in all samples increased TOY and the selectivity of light olefins, which indicated the tremendous effect of micro-meso-macroporous system in removing the products as quickly as possible, because more aromatic intermediates are produced, which turn into aromatics if the reaction continues, with the decrease of temperature and energy in the catalytic bed. However, the rapid exit and moderate acidity of samples lead to the production of olefins. All samples, except Mn-ZM, showed increased P/E ratio by decreasing the temperature, probably due to the greater conversion of aromatic intermediates to propylene. At 400 °C in Al-ZM and Ga-ZM, the passage of reaction time reduced the selectivity of light olefins, but the impressive performance of Ga-ZM showed that the longer the reaction time, the more propylene was produced, which reached P/E ≃ ∞ at 10th hour. In addition, TOY in these two samples did not obviously change during 10 hours. In MTO, Ga-ZM was introduced to produce more propene at 400 °C using a system that has the ability to run at high flow rates. The low production BTX in all samples also confirm rapid exit of products in this system.
Catalyst sample | Reactor productivity ideal value (>0.5) | Catalyst consumption ideal value (0.1>) | RHa | ||
---|---|---|---|---|---|
P | P + E | ∑olefins | Propylene | ||
a Required stability hours to observe ideal value for the catalyst consumption.13 | |||||
Ga-ZMMicro | 4 | 5.3 | 7 | 12.6 | 1260 |
Fe-ZMMicro | 3.3 | 4.3 | 5.6 | 15.1 | 1510 |
Mn-ZMMicro | 3.1 | 4.3 | 6 | 15.9 | 1590 |
Zn-ZMMicro | 3.2 | 4.5 | 5 | 15.7 | 1570 |
Al-ZMMicro | 4.2 | 5.3 | 7.9 | 11.8 | 1180 |
Al-ZMFixed-bed32 | 0.06 | 0.07 | 0.11 | 11.3 | 11300 |
The calculation of CC in 10 h showed that in order to achieve the ideal value of sustainable catalysis, at least Al-ZM must show 1180 h of stability in order to be introduced as an environmentally friendly catalyst. By contrast, the required stability for the same catalyst in the fixed-bed reactor is approximately 11300 h.
Al-ZM: for the purpose of propene and olefin production in HTO
Ga-ZM: for the purpose of propene production at 400 °C, and olefin production at 450 °C in MTO
Mn-ZM: for the purpose of propene production at 450 °C in MTO
Fe-ZM: for the purpose of olefin production at 400 °C in MTO
This journal is © The Royal Society of Chemistry 2023 |