Excessive tetracycline in the water environment may lead to the harming of human and ecosystem health. Removing tetracycline antibiotics from aqueous solution is currently a most urgent issue. Porous graphitic biochar with an ultra-large surface area was successfully prepared by a one-step method. The effects of activation temperature, activation time, and activator dosage on the structural changes of biochar were investigated by scanning electron microscopy, Brunauer–Emmett–Teller, X-ray powder diffraction, and Raman spectroscopy. The effect of the structure change, adsorption time, temperature, initial pH, and co-existing ions on the tetracycline removal efficiency was also investigated. The results show that temperature had the most potent effect on the specific surface area, pore structure, and extent of graphitization. The ultra-large surface area and pore structure of biochar are critical to the removal of tetracycline. The qe of porous graphitic biochar could reach 1122.2 mg g−1 at room temperature. The calculations of density functional theory indicate that π–π stacking interaction and p–π stacking interaction can enhance the tetracycline adsorption on the ultra-large surface area of graphitic biochar.
The application of biochar prepared from different biomass to remove TC has attracted extensive attention from scholars, such as alfalfa,13 bovine manure,14 maple leaf,15 and sludge,16 which exhibit excellent adsorption performance. The mechanisms responsible for TC adsorption by biochar could be assigned to hydrogen bonding, π–π interaction, and electrostatic.17 For example, Hussam et al.18 suggested that hydrogen bonding and π–π electron–acceptor–donor interactions are two fundamental adsorption mechanisms of the biochar from excess food and garden materials. They had an adsorption capacity between 2.98 mg g−1 and 8.23 mg g−1 for initial TC concentrations of 20 mg L−1 and 100 mg L−1, respectively. The mechanism of TC adsorption on rice straw-derived biochar mainly included physical adsorption, electrostatic interaction, hydrogen bonding, and π–π interaction, with the maximum adsorption capacity could reach 103 mg g−1.19 However, many pristine biochars have a low specific surface area, poorly formed pores, and graphitic structures.20 which leads to low adsorption performance (Qe < 150 mg g−1) without the possibility of practical application.9,18
In order to solve the structural problem of pristine biochar with low adsorption capacity, chemical activation has been used in the preparation process of biochar with ultra-surface area for exposing more adsorption sites. The material has an ultra-high specific surface area, which helps to improve its practical application performance-for example, the adsorption of iodine and catalytic styrene.21,22 Currently, biochar has been activated by FeCl3,23 H3PO4,24 and NaOH20 as the activating agent, to change its surface structure to improve the adsorption efficiency of TC. For example, Kan et al.25 prepared NaOH-activated biochar with high adsorption performance by activating alfalfa with NaOH. The specific surface area of biochar increased from 0.68 m2 g−1 to 796.50 m2 g−1, and the adsorption performance of tetracycline was improved from 17.85 to 232.88 mg g−1. The surface structure of biochar was markedly improved. However, biochar is inevitably post-treated with strong acid or strong alkali to remove the activating agent, increasing the process cost and second environmental pollution for adsorption TC. Therefore, there are two noteworthy points for selecting the activating agent in pyrolysis biomass: (1) easy to occur in the biochar surface reaction, increasing the pore structure and surface area. (2) No residue on the biochar surface, and easy to collect activating agents after the pyrolysis process. In this study, ZnCl2 is selected as activator, and its pore-forming process is as follows. Firstly, when the temperature reaches about 400 °C, ZnCl2 and H2O from the pyrolytic biomass start to transform to ZnO: ZnCl2 + H2O → ZnO + HCl.26,27 The pores formation begins after 600 °C. Secondly, the reaction of ZnO and the biochar from biomass form Zn and other gases. Lastly, in the process from liquid metal zinc to gaseous metal zinc at high temperature, porous can also be further made to increase the surface area of biochar, and metal Zn can be further collected: Zn (liquid) → Zn (gas).28 Therefore, ZnCl2 activating agents can prepare the porous and high surface area of biochar because there are two porous-making processes on biochar.
In this work, we select corn starch as the source of biochar because it is widely used and is an essential raw material in the food, chemical industry, medicine, and other industries. Especially there is a large surplus of genetically modified (GM) corn, and this work also can provide an application for GM corn.29 Corn starch and ZnCl2 can form a uniform mixture by the planetary ball mill machine to produce porous biochar by pyrolysis. The specific surface area, pore structure, and graphite degree of biochar were controlled by the activation temperature, dosage of ZnCl2, and activation time. The adsorption efficiency of TC on porous biochar was evaluated, including the pH, adsorption time, concentration of TC, adsorption temperature, and coexisting ions. The adsorption mechanism between biochar and TC will be proposed. It will be a new path for further research on developing the high-adsorption performance of tetracycline on porous graphitic biochar with an ultra-large surface area.
The cycle experiment process was as follows. Take 100 mg adsorbent and 500 mL tetracycline for adsorption. After one adsorption, collected the biochar and washed with deionized water, then dried at 80 °C. The TC-loaded biochar was desorbed with 0.1 M NaOH solution for 12 h and repeated the above experiment 5 times in a turn. The calculation of adsorption capacity, removal efficiency, kinetics, isotherms, and thermodynamics were presented in ESI (Table S2†).
Fig. 1 SEM image of samples: BC2-400-4 (a); BC2-600-4 (b); BC2-800-4 (c); BC2-1000-4 (d); BC1-800-4 (e); BC3-800-4 (f). |
BC800 has a bulk morphology under high temperatures (Fig. S1a†). BC2-400-4 and BC2-600-4 exhibit similar morphologies and sizes (Fig. 1a and b) to BC800 at activation temperatures of 400 °C and 600 °C, respectively. The results indicate that at lower activation temperatures, ZnCl2 has a weaker effect on the surface morphology and pore-forming ability of the biochar. However, at activation temperature of 800 °C and above, the biochar surface exhibits a distinct porous structure (Fig. 1c and d), indicating that high temperatures are favorable for generating pores and porous surface structures by ZnCl2 in biochar.30
The effect of activation time on the surface morphology of BC is shown in Fig. 1e and f. The porous surface cannot be obtained when the reaction activation time is 1 h at 800 °C. It is obvious that a shorter activation would not be beneficial to form a porous surface. When the reaction time is 2 h, the surface of the material exhibits a porous structure. However, the longer activation time via ZnCl2 above 3 h will lead to the collapse of the channel or even millimeter-sized pore on BC3-800-4 (Fig. 1f). The amount of ZnCl2 will also affect the surface structure, the ratio of ZnCl2/starch is lower than 2:1 at 800 °C, and the surface of the BC does not have porous structures in Fig. S1a–d.† Further increasing the ratio of ZnCl2/starch will show an obvious porous structure on the biochar, indicating that the amount of ZnCl2 can affect forming of the structure of the porous biochar with some millimeter-sized macropores.31 Overall, starch was treated with ZnCl2 (4:1, ZnCl2/starch) for 2 h at 800 °C, and a porous surface of BC could be obtained. The presence of a porous structure can increase the surface area of biochar.
In order to further investigate the effect of porous structure on the surface of the BC, nitrogen adsorption–desorption isotherms were used to measure the specific surface area and pore structure of BC (Fig. 2, S2, S3, and Table S3†).
According to the IUPAC report,32 the BC800 in Fig. 3 exhibits a Type I isotherm (Fig. S2†), which is typically obtained from microporous materials.33 Instead, BCx-y-z is observed in Fig. S2 and S3† to exhibit an ink bottle-like hysteresis loop, which is the H2 hysteresis loop for the Type IV(a) isothermal line.32 This is generally observed in mesoporous materials with non-rigid pore structures, where such porous materials have narrow necks and wider openings,34 which allow TC molecules to enter and exit the pores at different pressures, facilitating mass capture of TC molecules.32,34
In order to investigate the effect of preparation conditions on the adsorption properties of biochar and reveal the influence of structure on the adsorption properties, the biochar adsorption properties were evaluated by using antibiotic tetracycline as adsorbate (Fig. 2).
The effects of activation temperature, time, and the amount of the activator on the BCx-y-z specific surface area and pore diameter are shown in Fig. 2a and b, respectively. As depicted in Fig. 2a, increasing activation temperature from 400 °C to 800 °C and time from 1 to 3 h, the specific surface area and pore diameter of BCx-y-z also increased from 1342 to 1711 m2 g−1 and 1.54 to 4.84 nm (Table S3†), respectively, displaying a positive correlation. This result indicated that activation temperature and time are favorable for increasing the specific surface area and pore diameter of biochar. As shown in Fig. 2b, the ratio of ZnCl2/starch was improved from 0.5 to 2, and the specific surface area also can increase from 870 to 1521 m2 g−1 (Table S3†). Then increasing the ratio of ZnCl2/starch from 2 to 6, the surface area change was not obvious. This result indicated that excess ZnCl2 was not effectively involved in the activation process of biochar. Obtained different samples of BCx-y-z were used for TC adsorption, showing the best adsorption capacity of about 900.5 mg g−1 and the worst adsorption capacity of about 168.25 mg g−1 for BCx-y-z (Fig. S4†).
What is the reason for the difference in adsorption performance for TC on the surface of biochar? As shown in Fig. 2c, it is easy to find that the adsorption capacity increase with the increasing of special surface area. The specific surface area was increased from 870 m2 g−1 to 1707 m2 g−1 (Table S3†), and the adsorption performance was improved from 168.5 mg g−1 to 900.5 mg g−1 (Fig. S4†). The special surface area has doubled, while the adsorption performance has increased by 5.3 times. It indicates that the large specific surface area is beneficial to adsorb the contaminant.35 The high surface area of BC provides enormous accessible active sites for the adsorption of TC. As shown in Fig. 2d, the adsorption capacity of micropores is less than 700 mg g−1, while the adsorption capacity of mesopores is about 800 mg g−1 (Fig. S4†). It is different from the traditional understanding that micropores and mesopores are favorable for the adsorption of contaminants.35,36 The microporous and mesoporous structures on the surface of biochar aren't key factors for the adsorption of TC. Zhu et al.37 found that the presence of micropores has little effect on the adsorption of tetracycline, while Liu et al.38 demonstrated that the adsorption of tetracycline on mesoporous biochar is negatively impacted. In order to further clarify the influence of reaction conditions on the degree of graphitization and to further investigate how the fabrication condition affects the crystallographic structures of BC, we used XRD and Raman to investigate the structural change of BC (Fig. S5†).
The broad diffraction peak at 23.1° in the pattern of BC indicates the amorphous carbon structure of BC (Fig. S5a and b†).39 As the temperature increased, a new diffraction peak at 43.8° was shown in the curve of BC, which represent graphitic carbon.40 After the activation temperature is higher than 600 °C, the graphitization of the biochar can be easily observed in the spectrum. It is not difficult to find that both the activation time and the activation dose have little effect on the peak at 43.6° at 800 °C. Therefore, the most important factor affecting the graphitization of BC is the activation temperature.
Raman spectroscopy was used to measure the change in the degree of graphitization (Fig. S5c and d).† The Raman spectrum of BC shows two highlighted peaks D and G, which are due to the graphite lattice vibration mode and order/disorder in the graphite structure of BC.18 The peak D indicates disordered sp3-hybridized carbon atoms with vacancies, whereas the peak G represents the extension of sp2 atom pairs in the carbon atom ring.40 Raman ID/IG ratios are applied to assess the quality of carbon materials.41 It is easy to see that the value of ID/IG gradually decreases from 0.9371 to 0.7716 with the increase in activation temperature (Fig. S5c†). The increasing temperatures have a positive influence on forming ordered sp2-hybridized CC bonds, which implies the formation of the graphitic structure.42 The ID/IG ratios decreased from 0.8898 to 0.8085 (Fig. S5c†) under the same temperature when increasing activation time. After above 2 h, the ID/IG ratios presented a trend of slight decrease. ZnCl2 leads to a decrease in ID/IG ratio, but this effect is relatively small (Fig. S5d†). There is an aromatic ring in the tetracycline molecule, and the graphitization of BCx-y-z is beneficial to the π–π interaction, which improves the adsorption performance. The lower the ID/IG value, the higher of the graphitizable degree of carbon material.43 As shown in Table S3,† BC1-800-4 and BC2-400-4 have similar specific surface areas (1331 and 1342 m2 g−1), but the ID/IG value of BC1-800-4 (0.8898) is lower than that of BC2-400-4 (0.9371) (Fig. S5c†), indicating that BC1-800-4 has a higher degree of graphitization. From Fig. S4,† it can be seen that the adsorption capacity of TC on BC1-800-4 (746 mg g−1) is slightly higher than that on BC2-400-4 (695 mg g−1). The same result was obtained for BC3-400-4 and BC2-1000-4. This indicates that for biochar with similar specific surface areas, a higher degree of graphitization can slightly promote the adsorption of TC. As shown in Fig. 2c, with increasing the ID/IG value from 0.8018 to 0.9371, defects increased, and the adsorption capacity also was enhanced from 168.52 to 695.3 mg g−1. At this point, the material has a low specific surface area, which shows that the surface defects of biochar under a low specific surface area are beneficial to improve the adsorption capacity. Moreover, with the decrease of ID/IG value from 0.9371 to 0.7716, graphitization is enhanced and adsorption capacity is increased. At this point, the material has a high specific surface area, which shows that the graphitization of biochar surface under a high specific surface area is beneficial to improve the adsorption capacity.
The internal diffusion model was used to investigate the mechanism of adsorption kinetics further. It can be seen from Fig. S6† that the adsorption of TC to BC2-800-4 is divided into three stages: external diffusion, internal adsorption, and balance.43 The rate constant (Ki1 > 87 mg (g−1 min−1/2)) is the largest in the first stage (Table S4†), which is a rapid adsorption process. It is due to external diffusion, and TC molecules quickly combine with the adsorption sites on the outer surface of BC2-800-4 from the solution.9 Then, the effective adsorption site density on the adsorbent decreases in the second stage. TC molecules not only bind with the remaining adsorption sites, but also slowly diffuse into the pores of BC2-800-4.47 In the third stage, the adsorption reached equilibrium, and the adsorption reached saturation. All the C values are not zero for all stages. It indicates that intra-particle diffusion is not the controlling factor affecting adsorption in the kinetic process.48
In order to evaluate the properties of TC adsorbed by BC, the adsorbent in this work was compared with the reported BC-based adsorbents (Table S6†). For TC adsorbents, BC2-800-4 has a large specific surface area (1645 m2 g−1) and a high qmax value (1122.2 mg g−1). Other activated biochar materials prepared using activators such as NaOH have good adsorption effects.51 However, their high corrosiveness leads to high preparation costs.43 Compared with other biochar materials activated by ZnCl2 (e.g., Zn-BC),11 the adsorption capacity of TC is only 93.44 mg g−1. The simple synthesis of BC2-800-4 and its excellent adsorption performance have broad application promising applications. The only drawback is that the activation temperature is high and the energy consumption is high.
The specific surface area dropped sharply from 1645 m2 g−1 before adsorption to 512 m2 g−1 after adsorption, indicating that a large amount of TC occupies the surface and pores of BC2-800-4 (Fig. 5a).56 Through the analysis of pore structure, we can find that the pore size decreases from 4.37 nm to 3.82 nm (after adsorption), and the pore volume decreases from 1.72 m3 g−1 to 0.68 m3 g−1 (after adsorption) (Fig. 5b). This proves that TC is effectively adsorbed into the surface and pores of BC2-800-4.
The infrared spectra showed that the stretching vibration peak of the adsorbent at 3438 cm−1 was reduced to 3432 cm−1 (Fig. 5c). It indicates hydroxy protonation shifts due to electrostatic interaction and hydrogen bond formation between hydroxyl and amino groups of tetracycline and oxygen-containing functional groups of BC2-800-4.18,57 The peak at 1639 cm−1, which is the vibration of CC, also shifted after adsorption. It is attributed to the π–π conjugate effect between the π electron enrichment region of BC2-800-4 and the aromatic ring in TC molecule.58
In order to compare the π–π interaction with the hydrogen bond force, the BC was calcined again at 800 °C for 2 h to reduce the –OH content in the BC2-800-4 (Fig. 5d). The results show that the degree of graphitization is higher (ID/IG = 0.7802 < 0.8128) and the adsorption capacity increased from 867 mg g−1 to 911 mg g−1. This shows that the contribution of the hydroxyl group is weaker than that of π–π interaction.
All density functional theory (DFT) calculations in this work were performed using Gaussian 09 program package.59 A polarized continuum model based on solute electron density (PCM-SMD)60,61 was employed to simulate the solvent effect of aqueous solution. The dispersion corrections were computed with Grimme's D3 (BJ) method in optimization.62 Full geometry optimizations were operated to locate all of the stationary points, using B3LYP density functional theory method with 6-31G(d) basis set for all atoms,63,64 namely, B3LYP/6-31G(d). Unless mentioned otherwise, the relative energies (ΔG, kJ mol−1) are relative to the initial reactants obtained at the B3LYP/6-31G(d) + PCM-SMD (water) level in aqueous solution under experimental temperature and pressure (298.15 K and 1 atm).
DFT calculations were carried out to verify the adsorption of TC over BC (graphene sheet C42H16 terminated by hydrogen atoms). Analysis of the wave function indicates that the electron absorption corresponds to the transition from the ground to the first excited state and is mainly described by one-electron excitation from the highest occupied molecular orbital (HOMO) to the lowest unoccupied molecular orbital (LUMO). The HOMO and LUMO are delocalized over the entire CC bond of BC, as depicted in Fig. 6a. Obviously, the HOMO and LUMO are delocalized over the entire CC bond of the benzene ring and oxygen atom of –OH group for TC in Fig. 6b. Consequently, the lone pair electron on 2p orbital of carbon atoms for BC spontaneously matches with the 2p orbital of the oxygen atom and the benzene ring for TC, resulting in such strong π–π stacking interaction and p–π stacking interaction from CC bond of benzene ring for BC to CC bond of benzene ring for TC and to the oxygen atom of –OH group for TC in BC-TCa, but in the adsorption BC-TCb structure only strong π–π stacking interaction, as shown in Fig. 6c. The positive adsorption free energy −12.10 and −3.19 kJ mol−1 of BC-TCa and BC-TCb, respectively, indicates that the product tends to desorb from the BC adsorbent. The adsorption-free energy of BC-TCa is greater than that of BC-TCb, which indicates that strong π–π stacking interaction and p–π stacking interaction can enhance the adsorption effect from BC to TC, compared to π–π stacking interaction. This result is consistent with the experimental results.
Fig. 6 (a) and (b) The visualization of the characteristic molecular orbital for BC and TC, respectively. (c) The weak interaction of BC-TCa and BC-TCb visualized using Multiwfn software.65 (d) Optimized geometric structures of BC with the TC adsorption mode. |
In summary, the adsorption mechanism of TC in aqueous solutions by BC can be visualized as follows: (1) the special surface area and pore structure of BC is critical to the removal of TC. (2) The π–π stacking interaction and p–π stacking interaction play an important role in the adsorption of TC. (3) Electrostatic attraction and hydrogen bonding also play an indispensable role in the adsorption of TC.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ra00745f |