Open Access Article
This Open Access Article is licensed under a
Creative Commons Attribution 3.0 Unported Licence

N-Doped porous carbons obtained from chitosan and spent coffee as electrocatalysts with tuneable oxygen reduction reaction selectivity for H2O2 generation

Alexandra S. M. Wittmar*ab, Thaarmikaa Vigneswarana, Nikola Rankovićcd, Ulrich Hagemannbe, Nils Hartmannbe, Ricardo Martínez-Hincapiébc, Viktor Čolić*bc and Mathias Ulbrichtab
aLehrstuhl für Technische Chemie II, Universität Duisburg-Essen, Universitätsstr. 745141, Essen, Germany
bNETZ – NanoEnergieTechnikZentrum, CENIDE – Center for Nanointegration Duisburg-Essen, Carl-Benz-Str. 199, 47057 Duisburg, Germany. E-mail: alexandra.wittmar@uni-due.de
cElectrochemistry for Energy Conversion, Max-Planck Institute for Chemical Energy Conversion, Stiftstr. 34-36, 45470 Mülheim an der Ruhr, Germany,. E-mail: viktor.colic@cec.mpg.de
dFakultät für Chemie und Biochemie, Ruhr-Universität Bochum, Universitätsstraße 150, 44801 Bochum, Germany
eInterdisciplinary Center for Analytics on the Nanoscale (ICAN), University of Duisburg-Essen, Carl-Benz-Str. 199, 47057 Duisburg, Germany

Received 18th April 2023 , Accepted 10th July 2023

First published on 27th July 2023


Abstract

Nitrogen-containing porous carbons prepared by the pyrolysis of adequate biopolymer-based precursors have shown potential in several electrochemical energy-related applications. However, it is still of crucial interest to find the optimal precursors and process conditions which would allow the preparation of carbons with adequate porous structure as well as suitable nitrogen content and distribution of functional groups. In the present work we suggested a straightforward approach to prepare N-doped porous carbons by direct pyrolysis under nitrogen of chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee blends of different compositions and using KOH for simultaneous surface activation. The synthetized carbon materials were tested for the electrochemical oxygen reduction to hydrogen peroxide (H2O2). A higher fraction of chitosan in the precursor led to a decrease in meso- and nano-porosity of the formed porous carbons, while their activity towards H2O2 generation increased. The nitrogen species derived from chitosan seem to play a very important role. Out of the synthesized catalysts the one with the largest content of pyridinic nitrogen sites exhibited the highest faradaic efficiency. The faradaic efficiencies and current densities of the synthesized materials were comparable with the ones of other commercially available carbons obtained from less renewable precursors.


Introduction

Hydrogen peroxide (H2O2) is a valuable chemical1–3 with a wide variety of applications in industry, which include: pulp and textile bleaching,4 wastewater treatment,5 biomass upgrading via oxidation,6 semiconductor cleaning, detergent production, and others.7 Additionally, it is used in households around the world as a cheap yet powerful disinfectant, important for combating global pandemics.8 H2O2 has a high oxidation potential in a wide pH range,9 making it a suitable oxidant in a wide range of conditions.4,10 Consequently, the global production of H2O2 is steadily rising and has reached 5.5 million tons/year as of 2015,11 with a trend of further growth. Currently, H2O2 is produced on an industrial scale via the anthraquinone-mediated reduction of oxygen (O2) known as the autooxidation or AO-process for short.12 The main drawbacks of the AO-process are the excessive use of organic solvents, its complexity, and organic contamination of H2O2.11 Most use cases of H2O2, require aqueous solutions of up to 9% by weight.7 Alternative routes for H2O2 have been proposed, such as direct synthesis of H2O2 from H2 and O2, thereby eliminating the separation step in production. However, in practice, the gas mixture (H2/O2) needs to be diluted, in order to avoid the risk of explosion. Moreover, only pure O2 in excess can be used, but not air, hence, increasing costs of production and making upscaling difficult, at the current state of the art.13 Alternatively, the electrochemical reduction of O2 can generate H2O2 directly, avoiding the aforementioned issues.14 The O2 reduction reaction (ORR) can proceed via the two-electron pathway and generate H2O2, or alternatively via the four-electron pathway and generate water and electricity.7,15,16 The two-electron pathway is interesting as it generates H2O2 in an aqueous solution directly, eliminating the need for the separation of H2O2 and the risk of explosion.4 Recently, it has been demonstrated that with the use of a solid electrolyte, which requires acidic reaction conditions (e.g., Nafion-H®), a 20% by weight aqueous solution of H2O2 can be obtained.17 Such electrochemical devices offer the possibility of onsite production of H2O2.7

Nevertheless, the cost of electrochemical production of H2O2 is primarily influenced by the amount of electricity consumed per mol of H2O2. To make electrochemical production of H2O2 economical, the amount of electricity consumed per mol of H2O2 produced needs to be minimized.7 Cost reduction and efficient use of electricity is possible with a suitable cathode catalyst that is able to achieve high faradaic efficiencies over an extended period and at high current densities.18,19 Over the years, many catalyst materials were tested for the electrochemical H2O2 production, including: pure metal surfaces,20 various alloys,21 single atom catalysts22,23 and carbon-coated metal nanoparticles.24 The main issue with noble metal catalysts is their availability. Many are scarce and at the same time difficult to extract and scale.25 Additionally, even minute residues of heavy metals, such as mercury16 can be problematic in long-term applications in some fields, such as agriculture.

Organic waste and biomass, as nature-derived materials and being low cost and abundant, are recently and intensively studied for clean energy storage and conversion applications.26 Carbon materials can be produced from organic waste products, thereby providing a sustainable source of catalyst material.27 As the production of municipal waste increases,28 the topic of waste recycling and valorisation is crucial for enabling sustainable development.29 For instance, the recycling of waste from corn stover,30 oats husks,31 tire rubber,32 eggshells,33 sugarcane processing residue,34 bamboo35 and coffee waste36–38 have been considered as possible pathways to produce various carbon materials. Coffee waste, for example, is characterized by high organic content, in the form of polysaccharides, fatty and amino acids, polyphenols and various minerals.36 Therefore, the wide consumption of coffee39 coupled with its high organic content make it a suitable candidate precursor for carbon materials with variable properties, such as sustainable catalyst materials. Chitin is a naturally abundant polysaccharide, primarily found in crustaceans, with a similar structure and function to cellulose. Chitosan on the other hand, is a N-deacetylated derivative of chitin. Both chitin and chitosan possess a higher nitrogen content than synthetically substituted cellulose.40 High nitrogen content of chitosan coupled with its biodegradability, biocompatibility, and non-toxicity41 make chitosan an excellent starting material to produce nitrogen-doped (N-doped) carbons, especially since it is abundant and a by-product of the food industry.42 Recent work conducted by Khan et al., showed that chitosan, in the presence of a co-dopant, in this case graphitic nanoparticles, can enhance the selectivity of the chitosan derived N-doped carbon material towards the two-electron O2 reduction and generate peroxide.43 Chitosan-derived N-doped electrocatalysts obtained by direct pyrolysis of chitosan or chitosan/1,10-phenanthroline could successfully electrogenerate H2O2 in amounts high enough for its direct application in Fenton-based electrochemical water treatment.44 When such a catalyst is doped with Fe after the first pyrolysis step, a catalyst with improved Fe–Nx catalytic sites and high selectivity towards the 4e ORR can be obtained.45

In the present work, we studied the influence of the chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee ratio of blends and of the biopolymer[thin space (1/6-em)]:[thin space (1/6-em)]KOH ratio used for activation on the porous structure formation and chemical composition of a series of N-doped porous carbons obtained by pyrolysis. The synthetized carbon materials were tested in electrocatalytic processes, namely, the oxygen reduction to H2O2. The focus was set on developing a facile procedure, which enables the production of high surface area porous carbons which are able to favour the two-electron reaction pathway of the ORR. The complex correlations between the synthesis conditions, material characteristics and their efficiency to the H2O2 generation were discussed in depth.

Experimental section

Materials

Coffee arabica type was obtained from a local supermarket (Kaffee Gold, Markus Kaffee GmbH & Co. KG). Before further use, normal coffee brewing was simulated by using the coffee powder as follows: the mass of coffee filling 5 coffee spoons was inserted in a filter and 1.4 L boiling water were poured in order to extract the soluble matter. The obtained coffee waste was afterwards dried at 100 °C in a laboratory oven and stored dry.

For the preparation of the porous chitosan and of the chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee blend spheres, chitosan with medium molecular weight (100[thin space (1/6-em)]000–300[thin space (1/6-em)]000 g mol−1) from Acros Organics made from the shell of shrimps and crabs Pandalus borealis was used as received.

The ionic liquid (IL) 1-butyl-3-methylimidazolium acetate ([Bmim][OAc]) in BASF quality (≥95%) was also purchased from Sigma-Aldrich and used without further purification. Dimethyl sulfoxide (DMSO; analytical reagent; ≥99.5%) from VWR International was used as co-solvent for the polymer dissolution. The solvent mixture used for the biopolymer solutions preparation consisted in [Bmim][OAc][thin space (1/6-em)]:[thin space (1/6-em)]DMSO = 1[thin space (1/6-em)]:[thin space (1/6-em)]1 (wt[thin space (1/6-em)]:[thin space (1/6-em)]wt) ratio.

Other used chemicals include KOH analytical grade (VWR Chemicals) and HCl 37% Ph. Eur. (Carl Roth).

Preparation of the porous chitosan and chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee composites

A chitosan solution with the concentration of 3 wt% was prepared as follows: chitosan was dispersed in a mortar in the IL[thin space (1/6-em)]:[thin space (1/6-em)]DMSO = 1[thin space (1/6-em)]:[thin space (1/6-em)]1 mixture. The formed polymer dispersion was transferred to a closed flask and heated at 70 °C until the complete dissolution of the polymer. During the dissolution process the mixture was stirred several times in order to prevent polymer accumulation at the bottom of the flask. For the samples containing coffee, the desired coffee waste amount was homogenously dispersed in the chitosan solution. From the prepared chitosan solution or from the coffee dispersions in chitosan solution the chitosan and the chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee spheres were fabricated by dropping cum phase separation technique. Drops of about 3 mm diameter were dispensed using a syringe in a water coagulation bath. The obtained spheres were washed several times with water for the complete removal of the solvent. The ionic liquid and DMSO can afterwards be recovered from the coagulation bath.

Pyrolysis processes

The compositions and procedures shown in Table 1 have been used for the preparation of the N-doped carbons by pyrolysis from coffee waste and chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee composites. Ceramic combustion boats were filled with the biopolymer[thin space (1/6-em)]:[thin space (1/6-em)]KOH mixtures and then they were inserted in the middle of the glass tube of the pyrolysis furnace Heraeus Kelvitron S. To create the nitrogen atmosphere, this tube was then connected to the nitrogen circuit and flushed with nitrogen for about 15 minutes. The samples were pyrolyzed at 800 °C for two hours under continuous nitrogen flow. Afterwards the samples are left to cool for two hours under nitrogen to room temperature, the ceramic boat with the carbonized sample was removed from the furnace. For each type of sample 4 of 5 batches were prepared in order to produce enough material. The pyrolyzed materials were washed first with 0.1 N HCl solution in order to remove the KOH residuals and thereafter with deionized water until pH 6 was achieved, then dried and finally stored in closed snap-cap vials until further use.
Table 1 Composition of the precursors used in the pyrolysis processes
Sample name Biopolymer composition Biopolymer[thin space (1/6-em)]:[thin space (1/6-em)]KOH ratio Procedure
a Mixing = the coffee waste and KOH were milled together in a mortar.b Impregnation = the desired KOH quantity was dissolved in a small amount of water and the biopolymer was impregnated with this KOH solution, then it was dried in an oven at 100 °C.
S1 100% coffee 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5 Mixinga
S2 100% coffee 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5 Impregnationb
S3 Chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee = 4[thin space (1/6-em)]:[thin space (1/6-em)]1 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5 Impregnation
S4 Chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee = 2[thin space (1/6-em)]:[thin space (1/6-em)]1 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5 Impregnation
S5 100% chitosan 1[thin space (1/6-em)]:[thin space (1/6-em)]0.5 Impregnation
S6 Chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee = 2[thin space (1/6-em)]:[thin space (1/6-em)]1 1[thin space (1/6-em)]:[thin space (1/6-em)]1 Impregnation


Material characterization

The porosity of the carbonized samples was characterized by nitrogen adsorption using a Coulter SA 3100 surface analyser. Prior to the measurement the samples were degassed for 60 min at 120 °C and after weighing they were degassed again for 600 min at 50 °C. The analysis of the isotherms was done according to Brunauer, Emmett and Teller (BET) and Barrett, Joyner and Halenda (BJH) methods.

Scanning electron micrographs (SEM) of the N-doped carbon powders were recorded with an Apreo S Lo Vac from Thermo Fisher Scientific instrument. The samples were sputtered with Au/Pd (80/20) at 0.1 mbar and 300 mA until a 2–3 nm layer was obtained. Images with different magnifications were taken.

The relative amounts of C, H, N, O in the pyrolyzed samples were determined using a EURO EA Carbon–Hydrogen–Nitrogen–Oxygen (CHNO) elemental analyser from EURO VECTOR. Each sample was measured two times and the presented result represents the average of the two measurements.

The X-ray photoelectron spectroscopy (XPS) measurements were performed with an ULVAC-Phi 5000 Versaprobe II device with monochromatic Al Kα source under 45° angle with respect to the sample surface. The binding energies were corrected using the C 1s peak at 284.5 eV.

Raman spectroscopy measurements were performed using a Renishaw InViva Raman spectroscope with a 532 nm laser over a spectral range from 98 to 3200 Raman shift/cm−1.

Dispersions of the prepared carbon materials in 70% isopropanol–30% water have been obtained after treatment for 30 min in a sonication bath. The agglomerate size in dispersion, was determined by dynamic light scattering (DLS) method using a Particle Metrix Stabilizer heterodyne backscattering equipment.

For ToF-SIMS analysis powder materials had to be properly bonded to the sample holder in order to avoid damage of the analyzer. Here, each powder has been fixed on an aluminum plate using a piece of a double-sided adhesive Kapton tape (Plano GmbH). Powders were spread onto the top side of the adhesive tape using a spatula trying to yield a mostly fixed, preferentially closed and flat layer of the material. Prior to mounting the aluminium plates onto the sample holder of the ToF-SIMS instrument, loose powder was removed via turning each plate and carefully tapping it with the edges onto a collection tray. For reference measurements a bare Kapton tape has been mounted.

Depth profiling experiments of the surface-near region have been carried out at two distinct sets of parameters employing a ToF-SIMS 5–100 (IONTOF): (i) for qualitative analysis the following ion sources and parameters have been used: the primary ion gun operated in spectrometry mode with Bi+ primary ions at 15 kV was scanned in random mode at a field size of 100 × 100 μm2 and a digital raster of 128 × 128 pixels. Charge compensation was ensured employing a low energy electron flood gun and O2 gas flooding at an oxygen pressure of 2 × 10−6 mbar. The analyzer was operated in positive polarity and corrected in order to compensate for surface potential shifts. Depth profiling of the near-surface region via non-interlaced sputtering was carried out at an analysis-to-sputtering frame ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]1 using an O2+ ion source operated at a sputtering voltage of 500 V and a field size of 400 × 400 μm2. (ii) For semi-quantitative analysis the following ion sources and parameters have been employed: For analysis Bi3+ primary ions and O2 gas flooding at an oxygen pressure of 4 × 10−6 mbar were used. Otherwise the same setting and parameters for the primary ion gun, the analyzer and charge compensation as outlined above were chosen, cf. (i) non-interlaced co-sputtering was carried out at an analysis-to-sputtering frame ratio of 1[thin space (1/6-em)]:[thin space (1/6-em)]1 using a Cs+ and Xe+ ion source operated at a Cs+ duty cycle of 75%, a sputtering voltage of 500 V and a field size of 400 × 400 μm2.

Time-of-flight software corrections have been employed in data analysis. Only those regions with high total secondary ion intensity are selected for analysis, as this results in a significantly improved mass resolution. Also, for analysis of the near-surface region sputter time intervals of (i) 100–600 s and (ii) 100–500 s are chosen in order to account for transient effects in the initial sputtering time window.

Electrochemical measurements

Unless stated otherwise, all electrochemical measurements were done in a three-electrode electrochemical glass cell with a VSP-3e bipotentiostat (BioLogic, France) and a rotating ring-disk electrode (RRDE) rotator (PINE research model: AFMSRCE, USA). The counter electrode used was a glassy carbon rod (HTW Hochtemperatur-Werkstoffe GmbH), the reference electrode was a home-made reversible hydrogen electrode (RHE), and the working electrode was a RRDE (E6R1; Pine research, USA) consisting of a glassy carbon disk with an area of 0.196 cm2 and Pt ring with an area of 0.11 cm2. The RRDE had a collection efficiency N = 0.25. The electrolyte used was aqueous 0.1 M HClO4 prepared from 70% HClO4 (ROTIPURAN®Supra) by dilution with Milli-Q water (18.2 MΩ). The catalyst ink was prepared by suspending the catalyst powder in a solution containing 70% isopropanol (99.5%, Roth®), 29.6% Milli-Q water and 0.4% Nafion® (5 wt% Sigma-Aldrich®). The concentration was 2 mg mL−1; 10 μL of the dispersion was dropped onto a freshly polished disk and dried under inert atmosphere for 5 min. The catalyst loading in all experiments was 0.1 mg cm−2. Since the loading of the carbon catalysts can have a significant effect on their faradaic efficiencies,46,47 we have kept the loading constant throughout this manuscript. The solution resistance (Rs) was determined using electrochemical impedance spectroscopy (EIS) from 20 kHz to 1 Hz at the open circuit voltage with a sinus amplitude of 5 mV. The Nyquist plots and equivalent circuit used to analyse the pot are given in the ESI (Fig. SI4).

Before ORR activity was investigated, the Pt ring of the RRDE was electropolished with cyclic voltammetry (CV) by sweeping the potential between 0.059 and 1.5 V at a scan rate of 200 mV s−1 under argon saturation (Ar 5.0, Air Liquide) for 50 cycles. The catalyst surface deposited on the working electrode was pre-treated in an argon saturated solution with 5 cycles of CVs from 0 to 0.9 V. Thereafter, the electrolyte was purged with oxygen (O2, 4.0, Air Liquide) for 15 min before linear sweep voltammograms (LSVs) were recorded at a scan rate of 10 mV s−1, and a rotation speed of 1600 rpm from open circuit voltage to −0.2 V. To detect the H2O2 produced during ORR the Pt ring potential was fixed at 1.1 V. The faradaic efficiency (FE [%]) was calculated according to relation (eqn (1)):

 
image file: d3ra02587j-t1.tif(1)
IR denotes the ring current, ID the disk current and N the collection efficiency (0.25). The partial current density (jH2O2) was calculated as follows (eqn (2)):
 
image file: d3ra02587j-t2.tif(2)
A denotes the geometric surface area of the disk (0.196 cm2), all other terms have their usual meaning.

Results and discussion

The SEM micrographs of the carbon-based materials (Fig. 1) show that the biochars are constituted from larger chunks which exhibit an extensive network of interconnected macropores and some smaller particles. By increasing the magnification, as exemplified for the sample S1 (Fig. 2), it was observed that in addition to the macropores the bulk of the materials also possesses a network of meso- and nanopores which are responsible for the very high specific surface areas. With the increase of the chitosan ratio in the used precursor mixture, the proportion of the meso- and nanopores present in the carbonized materials decreases, a fact which agrees with the values of the measured specific surface areas (SBET ≈ 1500 m2 g−1 for pyrolyzed coffee, SBET ≈ 1350 m2 g−1 for pyrolyzed chitosan/coffee mixtures and SBET ≈ 500 m2 g−1 for pyrolyzed chitosan). These differences in the specific surface areas of the carbonized materials may also be a consequence of the differences in the porous structures of the biopolymeric precursors used: while the porous chitosan obtained by freeze-drying from hydrogels has generally a microporous cellular structure,48 the coffee waste, though more porous, exhibits a poorly developed mesoporosity.49 A higher KOH ratio in the precursor mixture seems to favour the formation of even higher specific surface areas. This agrees with the findings of Tseng et al.,50 who were able to demonstrate that by increasing the KOH/char ratio when a chemical activation is performed the micropore development will be favoured, leading to the formation of carbons with higher specific surface areas.
image file: d3ra02587j-f1.tif
Fig. 1 SEM micrographs and the specific surface area (from BET analysis) for the porous carbon-based samples. Note, the scale bars at the bottom right of the SE micrographs are 4 μm.

image file: d3ra02587j-f2.tif
Fig. 2 SEM micrographs at different magnifications for the sample S1. Note, the scale bars at the bottom right of the SE micrographs from left to right are 300, 20, 4 and 1 μm.

The agglomerate size in 70% isopropanol–30% water, relevant for the electrode preparation, was estimated to be between ca. 300 and 600 nm (see ESI Fig. SI5).

The Raman spectra of the N-doped carbons are presented in Fig. 3. All spectra contain the D and G peaks which are specific to the sp2 carbons.51


image file: d3ra02587j-f3.tif
Fig. 3 (a) Raman spectra of the various carbons obtained in the present work. (b) The calculated ID/IG ratios by 4 peak fitting.

The D band is assigned to the disordered type carbon and the G band corresponds to the sp2 hybridized carbon in the graphite lattice, thus, the intensity ratio ID/IG gives a measure to the disorder degree present in the carbon lattice.52

The disorder degree in the carbon lattice seems to be related to the nitrogen content in the carbon-based materials (Table 2). The samples with the highest nitrogen content (S5) and (S3) also exhibit the highest disorder degree. Exception seems to be the sample (S6) which exhibits high disorder but the nitrogen content is much lower. However, deconvolution of the broad signal peaks into multiple strongly overlapping bands can be done only with considerable statistical uncertainty, so these values need to be taken tentatively.53

Table 2 Elemental composition of the samples pyrolyzed 2 h at 800 °C, determined by CHNO and XPS analysis
Sample C [%] N [%] O [%]
CHNO XPS CHNO XPS CHNO XPS
S1 74.9 70.7 0.7 1.7 22.5
S2 77.5 84.7 0.2 1.3 13.0
S3 74.9 84.1 3 3.5 10.0
S4 67.7 65.6 0.7 1.6 24.9
S5 67 86.8 3.8 3.5 19.2 9.0
S6 57.9 68.2 1.7 1.9 20.1 23.2


Clearly, the nitrogen amount in the pyrolyzed materials is strongly dependent on the used precursors: the pyrolyzed chitosan contains the highest amount of nitrogen (Table 2). For some of the samples the oxygen could not be detected by CHNO method but was observed by XPS suggesting that there may be oxygen in the sample bound in complexes, which may be present in the samples as impurities. Note, the ratio of chitosan[thin space (1/6-em)]:[thin space (1/6-em)]coffee of the biopolymer used for the preparation of sample S3 is 4[thin space (1/6-em)]:[thin space (1/6-em)]1, i.e., higher than those used for sample S4, that is, 2[thin space (1/6-em)]:[thin space (1/6-em)]1, cf. Table 1.

Fig. 4 presents the N 1s XPS spectra of the nitrogen-doped carbons obtained in the frame of this work. As the position and the intensity of the N 1s peaks of the nitrogen-doped carbons prepared by thermal decomposition of biopolymer-based precursors may be affected by different configuration effects like hydrogenation, oxidation or protonation, the deconvolution of the spectra and the assignment of the peaks is difficult. The recorded spectra exhibited peaks around 398.5 eV, 400.2 eV, 400.6 eV and 402 eV which based on specialized literature assignments54,55 and according to our previous results56 were ascribed to the pyridinic nitrogen, pyrrolic nitrogen, hydrogenated nitrogen and protonated nitrogen, respectively. Additionally, the distribution of the nitrogen species within the analysed N-doped carbons is shown in Fig. 5.


image file: d3ra02587j-f4.tif
Fig. 4 N 1s XPS spectra of samples S1 (a) to S6 (f).

image file: d3ra02587j-f5.tif
Fig. 5 Nitrogen species distribution for the N-doped porous samples, obtained from XPS.

The XPS results confirmed that the materials prepared from precursors with a higher chitosan content contained higher amounts of total nitrogen trapped inside the carbon lattice. The relationship between certain nitrogen species and catalyst performance is discussed later in this work.

Since it is well-known that the presence of trace amounts of metals can influence the selectivity of carbon-based catalysts for the ORR,57–59 time-of-flight secondary ion mass spectrometry (ToF-SIMS) has been employed in order to analyze traces of transition metals within the catalytic powders, which, e.g., could stem from the natural precursor materials coffee and chitosan or from the preparation procedure in general,60,61 ToF-SIMS in this respect offers a high surface and detection sensitivity, which makes it well suited for ppm level metal analysis of surfaces and near-surface layers.

At first, near-surface analysis of samples S1 to S6 employing an O2+ ion source for sputtering has been performed. This ensures a particularly high sensitivity for the detection of electropositive elements, such as transition metals.62 As the matrix elements of the samples result in a rich and complex mass spectrum, the analysis here focuses on the lower mass range, i.e., on metals from the first transition series, in order to ensure proper peak identification. Note, this includes common trace elements in coffee and chitosan as reported in the literature.60,61 Table 3 lists respective secondary ion intensities normalized by the intensity of the C+ mass peak. Virtually no mass peaks of metals from the first transition series were detected on the Kapton tape reference sample.

Table 3 Normalized secondary ion intensities of N+, Si+, M+ mass peaks
Sample IN+/IC+ ISi+/IC+ ITi+/IC+ IV+/IC+ ICr+/IC+
S1 0.0092 40 0.25 0.0054 0.011
S2 0.0066 45 0.05 0.0031 0.003
S3 0.0217 37 0.27 0.0051 0.039
S4 0.0084 105 0.50 0.0028 0.037
S5 0.0187 31 0.22 0.0033 0.061
S6 0.0115 102 1.17 0.0094 0.075

Sample IMn+/IC+ IFe+/IC+ INi+/IC+ ICo+/IC+ ICu+/IC+
S1 0.074 1.45 0.034 0.0366 0.83
S2 0.033 0.82 0.011 0.0022 0.64
S3 0.071 1.07 0.021 0.0073 0.07
S4 0.107 0.76 0.010 0.0038 0.14
S5 0.015 1.20 0.017 0.0042 0.05
S6 0.114 1.47 0.017 0.0028 0.18


For further reference also normalized intensities of the N+ and Si+ mass peaks are shown in Table 3. These ion intensities show a reasonable linear relationship to the corresponding atomic ratios obtained from the XPS analysis (Table SI2), suggesting that matrix effects, which in many cases complicate the ToF-SIMS analysis, are weak.62,63 For this reason, the normalized secondary ion intensities here, in first approximation, are considered to represent a measure of the relative concentration ratios. In good agreement with the XPS data, the normalized intensity of the N+ mass peak shows an increasing trend with increasing chitosan content of the precursor material. As evident from the data, however, the normalized intensity of the mass peaks of most transition metals shows no clear correlation with the coffee to chitosan mixture ratio. One notable exception being the normalized intensity of the Cr+ mass peak, which increases with increasing chitosan content of the precursor material in S2–S5. Note, samples S2–S5 are prepared following the same overall procedure, cf. Table 1, hence no matrix effects as a result from varying preparation conditions are expected. Also, the samples prepared from 100% coffee, S1 and S2, yield a higher normalized intensity the Cu+ mass peak, when compared with S5, prepared from 100% chitosan, and S3, S4 and S6, prepared from material containing higher amounts of chitosan.

For semiquantitative MCs+ analysis complementary measurements employing a Cs+/Xe+ ion source has been carried out.64 This yields MCs+ secondary ions of the transition metals, M. Also Si in this analysis yields SiCs+ secondary ions. Respective secondary ion intensities of the SiCs+ mass peak are used for normalization. Generally, IMCs+/ISiCs+ intensity ratios are less affected by matrix effects and hence scale with corresponding relative concentration ratios M/Si.64 Unambiguous peak identification, however, is challenging in the higher mass range. Also mass interferences limit the analysis. The FeCs+ mass peak, for example, overlaps with the Si2Cs+ mass peak. Isotope patterns can help to identify such mass interferences and allow for proper peak identification. The intensities of SiCs+, 29SiCs+, 30SiCs+ mass peak, for example, are in good agreement with the natural isotope pattern of Si, which clearly allows one to identify the SiCs+ mass peak. Mass interferences, however, cannot generally be discerned and ruled out in the high mass range, particularly for monoisotopic elements, e.g., Mn and Co. For these reasons IMCs+/ISiCs+ intensity ratios here are considered as upper bounds. In order to calculate upper bounds of the concentration of the transition metals these intensity ratios are multiplied with the atomic concentration of Si from the corresponding XPS analysis, i.e. about 1 at%. Table 4 lists respective upper bounds of the transition metal concentrations for samples S2 and S5, which are prepared from 100% coffee and 100% chitosan, respectively. Most values are in the range 10–1000 ppm range. The upper bounds for Mn are close to 1 at%. No Mn is detected in the XPS analysis suggesting, as discussed above, that the Mn+ mass peak indeed significantly interferes with mass peaks of other secondary ion species, e.g., CsKO+.

Table 4 Upper bounds of the concentration of transition metals (ppm)
Sample Ti V Cr Mn Fe Ni Co Cu
S2 225 94 107 3080 771 525 70 565
S5 87 225 201 7260 680 465 17 750


As expected, ToF-SIMS analysis of the near-surface region of the catalytic materials reveals the presence of some metals of the first transition series, i.e., Ti, Cr, Fe, Ni and Cu are identified via their isotope patterns. Normalized intensities of the N+ and Si+ mass peaks show a reasonable linear relationship to the corresponding atomic ratios obtained from the XPS analysis, suggesting that (i) matrix effects are weak and (ii) normalized secondary ion intensities represent relative measures of the concentration ratios. In good agreement with the XPS data, the normalized intensity of the N+ mass peak shows an increasing trend with increasing chitosan content of the precursor material. Also, the normalized intensity of Cr+ mass peak correlates with the chitosan amount used in the precursor material and the normalized intensity of the Cu+ mass peak in the samples prepared from 100% coffee is significantly higher when compared with samples prepared from 100% chitosan. Otherwise no clear correlation between the normalized intensity of transition metal secondary ion mass peaks is evident from the data. Upper bounds of the concentration of transition metals as obtained from MCs+ measurements generally are in the range 10–1000 ppm. For Mn an upper bound ≫ 1.000 ppm is calculated. The Mn concentration, however, is expected to be well below this value, as no Mn is detected in the XPS measurements.

For further evaluation and best illustration, Fig. SI7A–I show correlation graphs, plots of the measured faradaic efficiency vs. the normalized metal secondary ion intensities IM+/IC+. We would like to note, that, the thus obtained data mostly do not seem to show a direct correlation with the faradaic efficiency. One exception being the data for Cr. The samples, however, appear to contain only very low amounts of Cr, cf. Table 4, i.e., when compared with the concentration of nitrogen groups, such as pyridinic nitrogen, cf. Fig. 5.

To determine the selectivity of N doped porous carbons towards 2-electron oxygen reduction to H2O2 rotating ring-disk electrode (RRDE) measurements were conducted and the results are presented in Fig. 6. Where Fig. 6a shows the CVs of each sample in an Ar saturated electrolyte from 0 to 0.9 V recorded at 100 mV s−1, done as a preconditioning step. Additionally, the CVs in the non-faradaic region allow the determination of the double layer capacitance (Cdl) of the various samples. While S1, S2 and S6 show higher surface areas (SBET) than S4, S3 and S5 (cf. Fig. 1), the CV response and Cdl are the same order of magnitude for all materials (Fig. SI1 and SI2). To determine the selectivity of N-doped porous carbons towards two-electron ORR to H2O2 RRDE measurements were conducted. Linear sweep voltammetry was used to study H2O2 formation in a O2 saturated electrolyte; the corresponding disk current which arises from the O2 reduction is shown in Fig. 6c (bottom), whereas the Pt ring current originates from oxidation of H2O2 (Fig. 6c, top). The faradaic efficiency of N-doped porous carbons at various potentials is presented in Fig. 6b. Out of the N-doped porous carbons tested, sample S6 showed the highest FE of 69 ± 2% at −0.2 V. This value is nearly 15% higher than that for samples S1 and S2 which were derived only from coffee (i.e., no chitosan used). Such a difference in the FE of the conversion to H2O2 suggests the importance of chitosan doping in the synthesis of carbon catalysts for H2O2 generation. Furthermore, the highest ring currents were achieved by S5, S4, S6 and S3, whereas lower ring currents were generated by S1 and S2.


image file: d3ra02587j-f6.tif
Fig. 6 Linear sweep voltammograms in 0.1 M HClO4 at 10 mV s−1 and 1600 rpm where (a) shows cyclic voltammograms in Ar-saturated 0.1 M HClO4 from 0 to 0.9 V before ORR, (b) shows the FE as a function of electrode potential in O2-saturated 0.1 M HClO4 and (c) shows the ring and disk currents in O2-saturated 0.1 M HClO4.

The existence of multiple nitrogen functional groups in the N-doped carbon material makes it difficult to decouple which catalytic sites are active during catalysis, and moreover under which conditions.65,66 Nonetheless, a quasi linear relationship between the amount of pyridinic nitrogen in our carbons and FE [%] was obtained as shown in Fig. 7.


image file: d3ra02587j-f7.tif
Fig. 7 Correlation between pyridinic nitrogen content (from XPS) and FE [%].

Effects of different nitrogen groups on the ORR have been studied with computational methods over the years, in an attempt to decouple the various effects different nitrogen groups have on the ORR. However, the focus of these studies was usually the four-electron pathway, and only recently the two-electron pathway has attracted more interest by researchers.67,68

Recent experimental work done by the groups of Strasser69,70 and Fornasiero71 has tried to shed more light on the complicated interface during ORR. By measuring the nitrogen content of the carbons before and after the ORR at different pH, it was observed that the amount of pyridinic nitrogen diminishes after the ORR in low pH. This observation was explained by a protonation effect that occurs on the pyridinic nitrogen atom which influences the ORR pathway, thus making pyridinic nitrogen active for the ORR to H2O2 in acidic pH, but not in neutral or basic pH, where other nitrogen functional groups have a more pronounced effect on the ORR pathway.69–71

Depending on the effective catalytic activity of pyridinic nitrogen on one hand and metal-containing structural entities on the other hand transition metals might well contribute to the overall catalytic performance of the samples.57,72 In view of the higher concentration of pyridinic nitrogen these species could dominate the catalytic performance of the samples prepared with the addition of chitosan. In addition, transition metals might explain the catalytic performance of those samples prepared from 100% coffee.

Table 5 summarizes the faradaic efficiencies and partial current densities of all tested samples at −0.2 V. Again, it is shown that the carbon samples that contained chitosan as a nitrogen source show higher faradaic efficiency. The faradaic efficiency might also correlate with the degree of disorder (cf. Fig. 3); a higher degree of disorder of the carbon lattice could lead a higher faradaic efficiency. Additionally, higher specific surface area suggests an improved accessibility of the active centres, which may also lead to improved electrocatalytic activity. On the other hand, the partial current densities per geometric surface area, jH2O2,geom which were calculated from eqn (2) do not show significant differences. When normalized per electrochemical surface area (ECSA) gained form the double layer charging experiments (Table S1), jH2O2,DL, we observe that S5 has a markedly higher partial current density, notably this carbon also has a low BET surface area.

Table 5 Faradaic efficiency and the partial current densities for H2O2 generation at −0.2 V of porous carbon-based samples
Sample FE @ −0.2 V [%] jH2O2,geom @ −0.2 V [mA cm−2] jH2O2,DL @ −0.2 V [μA cm−2] SBET [m2 g−1]
S1 55 ± 4 1.48 2.92 1594
S2 51 ± 3 1.70 2.74 1515
S3 58 ± 0.1 1.68 3.74 1354
S4 60 ± 3 1.84 3.00 1357
S5 63 ± 3 1.85 5.46 512
S6 69 ± 2 1.70 3.87 1677


While most applications of hydrogen peroxide require diluted solutions,73,74 it is still desirable to be able to achieve higher concentrations in real-world devices. However, this is highly dependent on the design of the cell.75 To gain insight into the long-term performance of our porous carbon materials we conducted bulk electrolysis experiments in a home-made H-cell on a gas diffusion layer as the substrate electrode (see ESI; Fig. SI6). Similarly, to our results in the three-electrode set up, samples S6 and S5 showed the best performance, with 1662.5 μmol mgcat−1 cm2 h−1 and 1757.5 μmol mgcat−1 cm2 h−1 of H2O2 produced, respectfully (Fig. SI3). The slight difference in total amount of H2O2 produced per catalyst loading could be explained by a difference in the electrochemical surface area of the samples.

The inversely proportional dependence of the selectivity for the two-electron pathway of SBET is at first glance in contrast to some previously observed effects for commercial carbon black materials, where micropore volume promoted the reaction18 (although it is well-known that mesopores also display a promoting effect76). However, the carbons investigated in that work did not contain a substantial amount of nitrogen groups, that is ca. 50–2000 ppm only, while the best performing carbons in this work contain several at% N (cf. Table 2), i.e., several orders of magnitude more. In this regard special attention needs to be paid to the nitrogen groups introduced by the addition of chitosan. The exact role of different nitrogen functionalities in carbon are still somewhat under debate.19 This is due to several factors, such as: the influence of even minor metal contamination,77,78 effects of loading,79 hydrophobicity,80 difficulty synthesizing carbons with a single site type, differences between as-synthesized materials and materials in operando, etc. Zhao et al.81 showed that the overall amount of N does not in itself determine ORR activity, but that pyridinic and quaternary N lead to a lower overpotential for ORR, although in their work they used the RDE and only observed the overall ORR. Sharifi et al.82 found that the four-electron process proceeded mostly on quaternary N, while pyridinic sites favoured the two-electron pathway on heat-treated N-doped multiwalled carbon nanotubes. Several other researchers also noted the positive effect of pyridinic nitrogen to improve the selectivity for the 2-electron process.10,71 DFT calculations by Chen et al.83 identify several types of graphitic-N sites as active for the four-electron process. Nonetheless, e.g., Artyushkova et al.54 have considered that pyrrolic N serves as an active site for the first step of the oxygen reduction reaction, while it was assumed that pyridinic N reduces H2O2 further to water but in a lower amount.

Conclusions

We observed that chitosan leads to a decrease in meso- and nano-porosity in pyrolyzed carbon materials obtained from composites with coffee waste. RRDE measurements, in turn, showed that the samples prepared with chitosan showed higher activity towards H2O2 generation. The best faradaic efficiency of the sample with the highest pyridinic nitrogen content seems to be the result of several favourable circumstances, such as nitrogen presence in the carbon lattice, relatively high content of the pyridinic species and a higher specific surface area. To summarize, we used an abundant, easily accessible and separable waste source to synthesize carbon materials of tuneable properties capable of promoting the two-electron ORR. The faradaic efficiencies and current densities are comparable to many commercial carbon materials,56 which are often obtained from less “green” sources, e.g., by the partial combustion of aromatic oils, coal char and ethylene from fossil fuel sources.

Author contributions

Alexandra S. M. Wittmar: supervision, conceptualization, investigation, formal analysis, validation, writing – original draft and introduction. Thaarmikaa Vigneswaran: investigation, formal analysis, validation. Nikola Ranković: investigation, formal analysis, validation, writing – original draft and introduction. Ulrich Hagemann: XPS & Raman spectroscopy: investigation, formal analysis, writing – review & editing Nils Hartmann: TOF-SIMS: investigation, formal analysis, writing. Ricardo Martínez-Hincapié: supervision, conceptualization, formal analysis, writing – review & editing. Viktor Čolić: conceptualization, supervision, writing – review & editing. Mathias Ulbricht: supervision, writing – review & editing.

Conflicts of interest

The authors declare that they have no conflicts of interest.

Acknowledgements

Open Access funding provided by the Max Planck Society. We gratefully acknowledge collaboration with Mrs Claudia Schenk (nitrogen adsorption measurements) and Mr Tobias Bochmann (SEM characterization) at the University of Duisburg-Essen. The authors acknowledge also the support from the Interdisciplinary Center for Analytics on the Nanoscale “(ICAN), a core facility at the University of Duisburg-Essen (DFG RIsources reference: RI_00313), funded by the German Research Foundation (Project No. 233512597 and 324659309). We would also like to thank Mr Marcel Nolte for his efforts during the completion of this manuscript.

References

  1. R. L. Myers, The 100 Most Important Chemical Compounds: A Reference Guide, Greenwood Press, 2007 Search PubMed .
  2. R. Ciriminna, L. Albanese, F. Meneguzzo and M. Pagliaro, ChemSusChem, 2016, 9, 3374–3381 CrossRef CAS PubMed .
  3. S. Siahrostami, Chem Catal., 2023, 3, 100568 CrossRef CAS .
  4. J. M. Campos-Martin, G. Blanco-Brieva and J. L. G. Fierro, Angew. Chem., Int. Ed., 2006, 45, 6962–6984 CrossRef CAS PubMed .
  5. S. O. Ganiyu, M. Zhou and C. A. Martínez-Huitle, Appl. Catal., B, 2018, 235, 103–129 CrossRef CAS .
  6. S. P. Teong, X. Li and Y. Zhang, Green Chem., 2019, 21, 5753–5780 RSC .
  7. S. Yang, A. Verdaguer-Casadevall, L. Arnarson, L. Silvioli, V. Čolić, R. Frydendal, J. Rossmeisl, I. Chorkendorff and I. E. L. Stephens, ACS Catal., 2018, 8, 4064–4081 CrossRef CAS .
  8. A. A. Caruso, A. Del Prete, A. I. Lazzarino, R. Capaldi and L. Grumetto, Infect. Control Hosp. Epidemiol., 2020, 41, 1360–1361 CrossRef .
  9. D. Pangotra, L.-I. Csepei, A. Roth, V. Sieber and L. Vieira, Green Chem., 2022, 24, 7931–7940 RSC .
  10. N. Wang, S. Ma, P. Zuo, J. Duan and B. Hou, Adv. Sci., 2021, 8, 2100076 CrossRef CAS .
  11. S. Ranganathan and V. Sieber, Catalysts, 2018, 8, 379 CrossRef .
  12. H. J. Rledl and G. Pfleiderer, US Pat., 2158525A, 1939 Search PubMed .
  13. R. J. Lewis and G. J. Hutchings, ChemCatChem, 2019, 11, 298–308 CrossRef CAS .
  14. I. Yamanaka, T. Onizawa, S. Takenaka and K. Otsuka, Angew. Chem., Int. Ed., 2003, 42, 3653–3655 CrossRef CAS PubMed .
  15. E. Lobyntseva, T. Kallio, N. Alexeyeva, K. Tammeveski and K. Kontturi, Electrochim. Acta, 2007, 52, 7262–7269 CrossRef CAS .
  16. S. Siahrostami, A. Verdaguer-Casadevall, M. Karamad, D. Deiana, P. Malacrida, B. Wickman, M. Escudero-Escribano, E. A. Paoli, R. Frydendal, T. W. Hansen, I. Chorkendorff, I. E. L. Stephens and J. Rossmeisl, Nat. Mater., 2013, 12, 1137–1143 CrossRef CAS PubMed .
  17. C. Xia, Y. Xia, P. Zhu, L. Fan and H. Wang, Sciences, 2019, 366, 226–231 CrossRef CAS .
  18. V. Čolić, S. Yang, Z. Révay, I. E. L. Stephens and I. Chorkendorff, Electrochim. Acta, 2018, 272, 192–202 CrossRef .
  19. H. W. Kim, V. J. Bukas, H. Park, S. Park, K. M. Diederichsen, J. Lim, Y. H. Cho, J. Kim, W. Kim, T. H. Han, J. Voss, A. C. Luntz and B. D. McCloskey, ACS Catal., 2020, 10, 852–863 CrossRef CAS .
  20. J. S. Jirkovský, M. Halasa and D. J. Schiffrin, Phys. Chem. Chem. Phys., 2010, 12, 8042–8053 RSC .
  21. E. Pizzutilo, O. Kasian, C. H. Choi, S. Cherevko, G. J. Hutchings, K. J. Mayrhofer and S. J. Freakley, Chem. Phys. Lett., 2017, 683, 436–442 CrossRef CAS .
  22. J. Xi, S. Yang, L. Silvioli, S. Cao, P. Liu, Q. Chen, Y. Zhao, H. Sun, J. N. Hansen, J.-P. B. Haraldsted, J. Kibsgaard, J. Rossmeisl, S. Bals, S. Wang and I. Chorkendorff, J. Catal., 2021, 393, 313–323 CrossRef CAS .
  23. Y. Sun, L. Silvioli, N. R. Sahraie, W. Ju, J. Li, A. Zitolo, S. Li, A. Bagger, L. Arnarson, X. Wang, T. Moeller, D. Bernsmeier, J. Rossmeisl, F. Jaouen and P. Strasser, J. Am. Chem. Soc., 2019, 141, 12372–12381 CrossRef CAS PubMed .
  24. A. Lenarda, M. Bevilacqua, C. Tavagnacco, L. Nasi, A. Criado and F. Vizza, et al., ChemSusChem, 2019, 12(8), 1664–1672 CrossRef CAS PubMed .
  25. C. J. Rhodes, Sci. Prog., 2019, 102, 304–350 CrossRef PubMed .
  26. B. Jaleh, A. Nasri, M. Eslamipanah, M. Nasrollahzadeh, J. H. Advani and P. Fornasiero, et al., J. Mater. Chem. A, 2023, 11(17), 9333–9382 RSC .
  27. A. Shetty, V. Molahalli, A. Sharma and G. Hegde, Catalysts, 2023, 13, 20 CrossRef CAS .
  28. D. M.-C. Chen, B. L. Bodirsky, T. Krueger, A. Mishra and A. Popp, Environ. Res. Lett., 2020, 15, 074021 CrossRef CAS .
  29. P. R. Yaashikaa, P. Senthil Kumar and S. Varjani, Bioresour. Technol., 2022, 343, 126126 CrossRef CAS PubMed .
  30. H. Yu, Y. Xu, J. Hou, S. Nie, S. Liu, Q. Wu, Y. Liu, Y. Liu and S. Yu, Ind. Crops Prod., 2020, 145, 111961 CrossRef CAS .
  31. T. Sar, V. H. Arifa, M. R. Hilmy, J. A. Ferreira, R. Wikandari, R. Millati and M. J. Taherzadeh, Biomass Convers. Biorefin., 2022 DOI:10.1007/s13399-022-02408-1 .
  32. Z. Derakhshan, M. T. Ghaneian, A. H. Mahvi, G. Oliveri Conti, M. Faramarzian, M. Dehghani and M. Ferrante, Environ. Res., 2017, 158, 462–469 CrossRef CAS PubMed .
  33. M. Baláž, Z. Bujňáková, M. Achimovičová, M. Tešinský and P. Baláž, Environ. Res., 2019, 170, 332–336 CrossRef .
  34. A. M. Shabbirahmed, D. Haldar, P. Dey, A. K. Patel, R. R. Singhania, C. D. Dong and M. K. Purkait, Environ. Sci. Pollut. Res., 2022, 29, 62785–62806 CrossRef CAS .
  35. K. Li, W. Chen, H. Yang, Y. Chen, S. Xia, M. Xia, X. Tu and H. Chen, Bioresour. Technol., 2019, 280, 260–268 CrossRef CAS .
  36. A. Cervera-Mata, M. Navarro-Alarcón, G. Delgado, S. Pastoriza, J. Montilla-Gómez, J. Llopis, C. Sánchez-González and J. Á. Rufián-Henares, Food Chem., 2019, 282, 1–8 CrossRef CAS .
  37. M. Li, W.-Y. Cheng, Y.-C. Li, H.-M. Wu, Y.-C. Wu, H.-W. Lu, S.-L. Cheng, L. Li, K.-C. Chang, H.-J. Liu, Y.-F. Lin, L.-Y. Lin and Y.-C. Lai, Nano Energy, 2021, 79, 105405 CrossRef CAS .
  38. R. Ravindran, C. Desmond, S. Jaiswal and A. K. Jaiswal, Bioresour. Technol. Rep., 2018, 3, 7–14 CrossRef .
  39. C. Ágoston, R. Urbán, O. Király, M. D. Griffiths, P. J. Rogers and Z. Demetrovics, Int. J. Ment. Health Addiction, 2018, 16, 981–999 CrossRef .
  40. M. N. V. Ravi Kumar, React. Funct. Polym., 2000, 46, 1–27 CrossRef .
  41. H. M. Ibrahim and E. M. R. E. Zairy, in Concepts, Compounds and the Alternatives of Antibacterials, ed. B. Varaprasad, IntechOpen, Rijeka, 2015, ch. 4,  DOI:10.5772/61300 .
  42. H. Amiri, M. Aghbashlo, M. Sharma, J. Gaffey, L. Manning, S. M. Moosavi Basri, J. F. Kennedy, V. K. Gupta and M. Tabatabaei, Nat. Food, 2022, 3, 822–828 CrossRef PubMed .
  43. A. Khan, M. Goepel, J. C. Colmenares and R. Gläser, ACS Sustainable Chem. Eng., 2020, 8, 4708–4727 CrossRef CAS .
  44. G. Daniel, Y. Zhang, S. Lanzalaco, F. Brombin, T. Kosmala and G. Granozzi, et al., ACS Sustainable Chem. Eng., 2020, 8(38), 14425–14440 CrossRef CAS .
  45. G. Daniel, T. Kosmala, F. Brombin, M. Mazzucato, A. Facchin and M. C. Dalconi, et al., Catalysts, 2021, 11(3), 390 CrossRef CAS .
  46. A. Schneider, L. Colmenares, Y. Seidel, Z. Jusys, B. Wickman and B. Kasemo, Phys. Chem. Chem. Phys., 2008, 10(14), 1931–1943 RSC .
  47. Y. E. Seidel, A. Schneider, Z. Jusys, B. Wickman, B. Kasemo and R. J. Behm, Faraday Discussions, 2009, 140, 167–184 RSC .
  48. S. Takeshita, S. Zhao, W. J. Malfait and M. M. Koebel, Angew. Chem., Int. Ed., 2021, 60, 9828–9851 CrossRef CAS PubMed .
  49. L. F. Ballesteros, J. A. Teixeira and S. I. Mussatto, Food Bioprocess Technol., 2014, 7, 3493–3503 CrossRef CAS .
  50. R.-L. Tseng, S.-K. Tseng, F.-C. Wu, C.-C. Hu and C.-C. Wang, J. Chin. Inst. Chem. Eng., 2008, 39, 37–47 CrossRef .
  51. A. C. Ferrari and J. Robertson, Phys. Rev. B: Condens. Matter Mater. Phys., 2000, 61, 14095–14107 CrossRef CAS .
  52. X. Chen and N. Ye, RSC Adv., 2017, 7, 34077–34085 RSC .
  53. A. Sadezky, H. Muckenhuber, H. Grothe, R. Niessner and U. Pöschl, Carbon, 2005, 43(8), 1731–1742 CrossRef CAS .
  54. K. Artyushkova, J. Vac. Sci. Technol., A, 2020, 38, 031002 CrossRef CAS .
  55. P. Lazar, R. Mach and M. Otyepka, J. Phys. Chem. C, 2019, 123, 10695–10702 CrossRef CAS .
  56. A. S. M. Wittmar, M. Ropertz, M. Braun, U. Hagemann, C. Andronescu and M. Ulbricht, Polym. Bull., 2023, 80, 7827–7845 CrossRef CAS .
  57. L. Wang, A. Ambrosi and M. Pumera, Angew. Chem., Int. Ed. Engl., 2013, 52(51), 13818–13821 CrossRef CAS PubMed .
  58. J. Masa, A. Zhao, W. Xia, Z. Sun, B. Mei and M. Muhler, et al., Electrochem. Commun., 2013, 34, 113–116 CrossRef CAS .
  59. J. Masa, W. Xia, M. Muhler and W. Schuhmann, Angew. Chem., Int. Ed. Engl., 2015, 54(35), 10102–10120 CrossRef CAS PubMed .
  60. G. Adler, A. Nędzarek and A. Tórz, Slovenian J. Public Health, 2019, 58(4), 187–193 CrossRef PubMed .
  61. M. Grembecka, E. Malinowska and P. Szefer, Sci. Total. Environ., 2007, 383(1), 59–69 CrossRef CAS PubMed .
  62. N. Hartmann, ICAN Notes, 2020, vol. 1, pp. 1–2 Search PubMed .
  63. M. P. Seah and A. G. Shard, Appl. Surf. Sci., 2018, 439, 605–611 CrossRef CAS .
  64. K. Wittmaack, Surf. Sci., 2012, 606(3), L18–L21 CrossRef CAS .
  65. J. Zhang, H. Zhang, M.-J. Cheng and Q. Lu, Small, 2020, 16, 1902845 CrossRef CAS PubMed .
  66. Y. Ding, W. Zhou, J. Gao, F. Sun and G. Zhao, Adv. Mater. Interfaces, 2021, 8, 2002091 CrossRef CAS .
  67. K. Wan, Z.-p. Yu, X.-h. Li, M.-y. Liu, G. Yang, J.-h. Piao and Z.-x. Liang, ACS Catal., 2015, 5, 4325–4332 CrossRef CAS .
  68. C. Xia, J. Y. Kim and H. Wang, Nat. Catal., 2020, 3, 605–607 CrossRef CAS .
  69. Y. Sun, S. Li, Z. P. Jovanov, D. Bernsmeier, H. Wang, B. Paul, X. Wang, S. Kühl and P. Strasser, ChemSusChem, 2018, 11, 3388–3395 CrossRef CAS PubMed .
  70. Y. Sun, I. Sinev, W. Ju, A. Bergmann, S. Dresp, S. Kühl, C. Spöri, H. Schmies, H. Wang, D. Bernsmeier, B. Paul, R. Schmack, R. Kraehnert, B. Roldan Cuenya and P. Strasser, ACS Catal., 2018, 8, 2844–2856 CrossRef CAS .
  71. D. Iglesias, A. Giuliani, M. Melchionna, S. Marchesan, A. Criado, L. Nasi, M. Bevilacqua, C. Tavagnacco, F. Vizza, M. Prato and P. Fornasiero, Chem, 2018, 4, 106–123 CAS .
  72. L. Wang, Z. Sofer and M. Pumera, ACS Nano, 2020, 14(1), 21–25 CrossRef CAS .
  73. B. Puértolas, A. K. Hill, T. García, B. Solsona and L. Torrente-Murciano, Catal. Today, 2015, 248, 115–127 CrossRef .
  74. J. K. Edwards, S. J. Freakley, R. J. Lewis, J. C. Pritchard and G. J. Hutchings, Catal. Today, 2015, 248, 3–9 CrossRef CAS .
  75. J. Filippi, H. A. Miller, L. Nasi, M. V. Pagliaro, A. Marchionni and M. Melchionna, et al., Mater. Today Energy, 2022, 29, 101092 CrossRef CAS .
  76. M. Mazzucato and C. Durante, Curr. Opin. Electrochem., 2022, 35, 101051 CrossRef CAS .
  77. J. Masa, A. Zhao, W. Xia, Z. Sun, B. Mei, M. Muhler and W. Schuhmann, Electrochem. Commun., 2013, 34, 113–116 CrossRef CAS .
  78. J. Masa, W. Xia, M. Muhler and W. Schuhmann, Angew. Chem., Int. Ed., 2015, 54, 10102–10120 CrossRef CAS PubMed .
  79. E. J. Biddinger, D. v. Deak, D. Singh, H. Marsh, B. Tan, D. S. Knapke and U. S. Ozkan, J. Electrochem. Soc., 2011, 158, B402 CrossRef CAS .
  80. B. W. Noffke, Q. Li, K. Raghavachari and L.-s. Li, J. Am. Chem. Soc., 2016, 138, 13923–13929 CrossRef CAS PubMed .
  81. A. Zhao, J. Masa, M. Muhler, W. Schuhmann and W. Xia, Electrochim. Acta, 2013, 98, 139–145 CrossRef CAS .
  82. T. Sharifi, G. Hu, X. Jia and T. Wågberg, ACS Nano, 2012, 6, 8904–8912 CrossRef CAS .
  83. M.-F. Chen, T.-H. Chao, M.-H. Shen, Q. Lu and M.-J. Cheng, J. Phys. Chem. C, 2020, 124, 25675–25685 CrossRef CAS .

Footnote

Electronic supplementary information (ESI) available: Electrochemical active surface area determination, solution resistance determination, particle size determination, correlation graphs: faradaic efficiencies vs. normalized secondary ion intensities, bulk electrolysis method and result summary, H2O2 determination. See DOI: https://doi.org/10.1039/d3ra02587j

This journal is © The Royal Society of Chemistry 2023