Chiu Ling Onga,
Yew Chong Laib,
Thorsten Heidelbergc,
Wai Kit Tangc,
Vannajan Sanghiran Leed,
Nader Ghaffari Khaligha and
Joon Ching Juan*ae
aNanotechnology and Catalysis Research Centre, Level 3, Block A, Institute for Advanced Studies, University of Malaya, 50603, Kuala Lumpur, Malaysia. E-mail: jcjuan@um.edu.my
bOleon Port Klang Sdn. Bhd., 57, Jln Sungai Pinang 4/3, Taman Perindustrian Pulau Indah, 42920 Pelabuhan Klang, Selangor, Malaysia
cDepartment of Chemistry, Faculty of Science, University of Malaya, 50603 Kuala Lumpur, Malaysia
dDepartment of Chemistry, Centre of Theoretical and Computational Physics (CTCP), Faculty of Science, University of Malaya, 50603, Kuala Lumpur, Malaysia
eFaculty of Engineering, Technology and Built Environment, UCSI University, Cheras, 56000, Kuala Lumpur, Malaysia
First published on 19th October 2023
The conventional medium chain chlorinated paraffin (MCCP) and zinc dialkyl dithiophosphate (ZDDP) additives have greatly enhanced the extreme pressure (EP) and anti-wear (AW) performance of the metalworking fluids. However, chlorine- and zinc-containing additives are restricted in use due to eco-toxicity issue. Herein, ashless and non-corrosive dimercaptobenzothiadiazole derivatives, namely bis-2,5-benzylsulfanyl-[1,3,4]thiadiazole (BBST) and bis-2,5-octylsulfanyl-[1,3,4]thiadiazole (BOST) consist of three sulfur atoms have been synthesized and evaluated. The performance of BBST shows a weld load (PD) of 3089 N and AW value of 5 mm2, which represents an improvement of 3.1 and 7.4 folds over naphthenic base oil (NBO). In addition, BBST also outperformed BOST, MCCP, and ZDDP in terms of its weld load and AW properties. Based on XPS analysis and molecular electrostatic potential maps (MEPS), BBST exhibits superior tribology performance due to the interaction between the sulfur (S), nitrogen (N), and π-electrons of the benzene ring with the metal surface. The formation of FeS, Fe2O3 and Fe⋯N coordinate bonds contributes to the creation of an excellent tribofilm.
Metalworking fluids (MWFs) are commonly employed in industrial machining to cool and lubricate the contact region between metal workpiece.3 The extreme pressure (EP) and anti-wear (AW) additives are the main components in MWFs. The EP and AW additives interact thermo-chemically and tribo-chemically with the metallic surface, generating a tribo-film that shields the metal surface from further wear and welding.4,5 The commonly used MWFs EP and AW additives are chlorine-, phosphorus-, and sulfur-based additives.6 Nonetheless, chlorine-based additives are being discussed to be added as the restricted in use by the REACH (Registration, Evaluation, Authorization and Restriction of Chemicals) to reduce chemical eco-toxicity of consumer products,7,8 while the phosphorus-based additives have lower EP performance than that of chlorine- and sulfur-based additives, respectively.6
Presently, organo-sulfur is the most vital lubricant additive owing to its excellent EP and AW performance.9 Moreover, sulfur element is also greener than phosphorus and chlorine elements.10,11 Among the variety of sulfur-containing compounds, organo-sulfides, or polysulfides, including sulfurized isobutene, dialkylpentasulfide, and di(iso-butyl) polysulfide have been commercialized as EP lubricant additives owing to their excellent load-carrying capacity. Their weld load performance is up to 7000 N because of high sulfur content (n = 5). Nevertheless, an excessive amount of sulfur content can lead to significant problems with metal corrosion and increased wear rate on the metal surface. This can ultimately result in decreased AW performance.12,13 In addition, polysulfides additives are also highly corrosive to the copper-based alloy. It was reported that the number of sulfur exceed three atoms a molecule will potentially induce corrosion.14 Therefore, the development of ashless, non-corrosive, high EP, and AW sulfur-based additives has attracted the interest of researchers.
Heterocyclic organic compounds, including derivatives of dimercaptobenzothiadiazole, have been identified as effective additives for lubrication. They offer excellent extreme pressure (EP) and anti-corrosion properties as well as thermal stability when used in polar base oils like rapeseed oil and trimethylolpropane trioleate.15–18 Besides, the compact molecular structure of dimercaptobenzothiadiazole with rich sulfur and nitrogen atoms can easily interact with the metal surface to generate a stable adsorption tribo-film.19 Moreover, the nitrogen elements also improve the biodegradability of friction modifiers and provide sufficient nutrients to microorganisms. Dimercaptobenzothiadiazole is also “ash-free” and “phosphorus-free” which meets the environmental protection regulations.20,21 Dimercaptobenzohiadiazole derivatives with three sulfur atoms are highly effective in EP performance. However, the high sulfur content in these compounds can also result in metal corrosion.22–26 Additionally, the dimercaptobenzothiadiazole derivatives also shows poor solubility in non-polar base oils, which limits their application as lubricant additives.17,24
The polarity of the base oil is a crucial factor in determining the thickness and growth rate of the tribofilm layer created by the additives.27 When mixed with non-polar base oils, additives produce a thicker tribofilm due to the lower affinity of base oil molecules to react with the metal surface. This results in increased affinity of additive molecules to react with the metal surface and create a protective tribofilm. Additionally, the compatibility between the base oil and additive is crucial for improving lubrication performance.28 An additive with good solubilty can increase the absorptivity of additives on the metal surface, leading to better tribological performance. Since naphthenic base oil (NBO) is non-polar, low aromatic content, high viscosity, better-emulsified ability, low pour point, and compatible with most additives,29 it is commonly used as MWFs base stock.
Our previous work30 found that disulfide functionalized by alkyl and benzyl groups are completely soluble in NBO and non-corrosive (grade 1a). Besides, the EP and AW performance of disulfide derivatives was also better than MCCP and ZDDP, respectively. Thus, the tribology performance of alkyl- and benzyl-substituted dimercaptobenzothiadiazole derivatives on NBO are worth investigating due to different characteristics. The exploration between the chemical structure and solubility, EP, AW, and corrosiveness performance is necessary to provide the basic understanding.
In this work, a more environmentally friendly and ashless dimercaptobenzothiadiazole additives, namely bis-2,5-benzylsulfanyl-[1,3,4]thiadiazole (BBST) and bis-2,5-octylsulfanyl-[1,3,4]thiadiazole (BOST) were synthesized and used as multifunctional lubricant additives in the NBO. The solubility, corrosiveness, EP, and AW performance of the dimercaptobenzothiadiazole derivatives in NBO were studied.
The chemical structure of the synthesized dimercaptobenzothiadiazole additives was confirmed by nuclear magnetic resonance (Brüker Avance III, 600 MHz), Agilent 6560 iFunnel Q-TOF LC-MS, and Agilent 6890N GC-MS. The spectra data were provided in ESI data Fig. S1 and S2.†
Table 1 provides the density and viscosity for NBO, 10 wt% BBST, and 10 wt% BOST at three different temperatures (25 °C, 40 °C, and 100 °C). It is apparent that 10 wt% BBST (150.2) has a higher viscosity index (VI) compared to BOST (123.7). This indicated that BBST can form a thicker boundary lubrication film to protect the metal surface than that of BOST.34 The VI values are ranked as BOST < BBST < NBO. Fig. S4† depicted that the dynamic viscosity of NBO and 10 wt% additives decreased as the temperature increased.
Lubricant | NBO | BBST | BOST | |
---|---|---|---|---|
Density (g mL−1) | 25 °C | 0.9427 | 0.7872 | 0.8954 |
40 °C | 0.9423 | 0.7868 | 0.8939 | |
100 °C | 0.9408 | 0.7848 | 0.8920 | |
Dynamic viscosity (mPa s) | 25 °C | 31.50 | 44 | 42.00 |
40 °C | 22.50 | 23 | 21.50 | |
100 °C | 5.50 | 5.00 | 4.50 | |
Kinematic viscosity (mm2 s−1) | 25 °C | 36.79 | 55.89 | 46.91 |
40 °C | 26.28 | 29.23 | 24.05 | |
100 °C | 6.42 | 3.82 | 2.80 | |
Viscosity index | 213.0 | 150.2 | 123.7 |
Fig. 1 shows the thermal stability of the BBST, BOST, MCCP, and ZDDP. The initial decomposition temperature (Td) of BBST, BOST, MCCP, and ZDDP are 284.69 °C, 281.19 °C, 217 °C, and 217 °C, respectively. The initial thermal degradation temperature of the BBST (284.69 °C) is higher than BOST (281.19 °C) might be due to the electronic delocalization and rigidity of the benzene ring in BBST. Lizarraga et al.35 reported that the urea and selenourea compounds containing aromatic substituents have higher initial decomposition temperature than those with aliphatic groups due to rigidity and electronic delocalization in the π orbitals of the aromatic ring. Besides, the initial thermal degradation temperature of the aromatic polyesters is higher than that of aliphatic polyesters presumably to the rigidity of the aromatic structures.36 However, the aromatic substituted polyesters are still decomposed faster than aliphatic substituted polyesters at temperature above 500 °C.
Furthermore, both BBST and BOST are more thermally stable than that of MCCP and ZDDP because of their high Td. Furthermore, the Td for 50% and 80% weight loss of BBST (295.54 °C and 302.38 °C) is lower than BOST (310.36 °C and 321.34 °C), which indicates that BBST has lower thermal stability than that of BOST. Therefore, it is presumably that BBST decomposes faster than that of BOST and thus the S and N active elements have higher affinity to react with the metal surface and generate a tribofilm. Other studies37 also observed that additives with lower decomposition temperature has higher activity to react with the metal surface and generate a protective layer. Besides, the TG curve also showed that the BBST and BOST almost completely decomposed above 592 °C without any ash remaining. However, we observe that even after 500 °C, the ZDDP left around 30% solid ash due to its Zn content. Both BBST and BOST are more environmentally benign than ZDDP due to heavy metal-free. Besides, the ashless properties also prevent suspended formation and minimize the damage to the machine during operation.
The corrosion grade of NBO, 10 wt% BBST, 10 wt% BOST, 10 wt% MCCP, and 10 wt% ZDDP are shown in Fig. 2. The copper strip of NBO appears as the freshly polished strip, which is grade 1a. The copper strips of BBST and BOST appear in light orange, which is also grade 1a. Nonetheless, the copper strips of MCCP and ZDDP exhibited mild discoloration (deep orange, 1b) after the test, which indicated that MCCP and ZDDP are corrosive to copper-based material.
The inhibiting mechanism of BBST and BOST can be ascribed to the adsorption of dimercaptobenzothiadiazole molecules on the metal surface.38,39 The adsorption mechanism of dimercaptobenzothiadiazole derivatives can be attributed to the interaction between the S and N elements present in the dimercaptobenzothiadiazole ring with the metal surfaces. The interaction between the lone pair electron in the N elements of the dimercaptobenzothiadiazole ring and the π electron in CN double bond, known as P–π conjugation, plays a crucial role in enhancing the adsorption of dimercaptobenzothiadiazole derivatives onto the metal surface. Furthermore, the adsorption efficiency of BBST is higher than that of BOST due to the presence of benzene ring. The π bonds of the benzene ring in BBST can interact with the empty d-orbital of metal atoms, resulting in the formation of a more stable adsorption film. Conversely, the long carbon chains in BOST tend to align horizontally to cover more copper surface which protect metal surface from corrosion. Another study also observed that π electron in benzene rings, CN bond, long carbon chains, S, and N elements can effectively formed a stable adsorption film to protect the metal surface.38,40
As previously stated, the bonding between dimercaptobenzothiadiazole derivatives and metal surfaces occurs via electrostatic interaction between the S and N atoms in the dimercaptobenzothiadiazole ring and metal surfaces, resulting in the formation of coordinated bonds between S and N atoms with metal surfaces.41,42 In case of BBST, the presence of a benzene ring enhances its adsorption efficiency to metal surface than BOST due to the π-electron interactions. Therefore, the S and N element in the BBST has a higher affinity to react with the metal surface. Besides, as observed earlier, BBST also has lower thermal stability than BOST. Consequently, BBST decomposes faster than that of BOST and thus allows more S and N elements to coordinately react with the metal surface to produce a high-melting point and low-shear strength metal salt film.
Fig. 4 shows the maximum non-seizure load (PB) and weld load (PD) of NBO with different concentration additives. Fig. 4 shows the initial PB and PD value of NBO are 785 N and 981 N, respectively. The results show that 10 wt% BBST has significantly improved the PB value (2452 N) and PD (3089 N) of NBO, which was 3.13 times that of NBO. While the PB and PD value of BOST reached 1961 N and 2452 N, which was 2.5 times that of NBO. This implies that both BBST and BOST can greatly enhance the load-carrying ability of NBO, and the PB and PD value of the NBO improved as the concentration of the additives increased. The BBST exhibited higher PB and PD than that of BOST.
The PB and PD value of the synthesized additives was also compared with commercial additives, such as MCCP and ZDDP. The PB and PD value of 10 wt% MCCP 1961 N and 2452 N, whereas 10 wt% ZDDP gives 1236 N and 1569 N, respectively. Both the BBST and BOST have higher EP performance than that of MCCP and ZDDP. The EP performance of the additives is ranked as BBST > BOST > MCCP > ZDDP.
As mentioned earlier, BBST has lower thermal stability than BOST. Thereby, it is presumably that the BBST is more easily decomposed than that of BOST and thus allow more S and N active elements to be absorbed on the metal surface to form an anti-seizure layer. The AW and EP performance of BBST and BOST is also in good agreement with their thermal stability.
Fig. 5 SEM images of the wear scars on the test cylindrical with 10 wt% (a) NBO, (b) BBST, (c) BOST, (d) MCCP, and (e) ZDDP in NBO. |
Furthermore, the elemental composition of the worn surfaces lubricated with 10 wt% BBST and 10 wt% BOST shows the presence of S and N elements (Table 2 and Fig.S5†). The S and N contents deposited on the worn surfaces from BBST are 1.4 and 0.2 wt%, which is 70.0 and 66.7% higher than that of BOST. The worn surfaces of MCCP show the presence of Cl, whereas the ZDDP shows the presence of P, S, and Zn. The composition on the worn surfaces is in good agreement with their AW performance.
Sample | EDX analysis (wt%) | |||||||
---|---|---|---|---|---|---|---|---|
C | Fe | O | S | N | Cl | Zn | P | |
NBO | 8.5 | 90.1 | 1.4 | — | — | — | — | — |
BBST | 9.7 | 86.7 | 2.0 | 1.4 | 0.2 | — | — | — |
BOST | 7.7 | 90.0 | 1.6 | 0.6 | 0.1 | — | — | — |
MCCP | 10.0 | 85.9 | 3.7 | — | — | 0.4 | — | — |
ZDDP | 9.0 | 87.2 | 1.6 | 1.0 | — | — | 0.7 | 0.5 |
Fig. 6(a) shows the results of the Fe 2p, S 2p, N 1s, and O 1s spectra obtained from the XPS analysis when lubricated with 10 wt% of BBST in NBO. From Fig. 6(a), the Fe 2p absorption peak at 710.1 and 723.7 eV belongs to Fe2+. In addition, the binding energy difference was 13.6 which is similar to reference iron sulfide (FeS).43 The Fe 2p peaks at 712.2 and 725.2 eV corresponded to the iron sulfate (FeSO4) and iron(III) oxide (Fe2O3), and combined with the O 1s peak around 529.7 and 531.5 eV and S 2p peak around 168.4 eV, the existence of Fe2O3 and FeSO4 could be validated.44 The S 2p peak appeared at 160.9, 162.5, 161.9 and 164.2 eV correspond to sulfide.43–45 In the spectrum of N 1s, the peaks at 398.7 and 400.0 eV are attributed to CN and Fe⋯N coordinate bonds.44 These results confirm that tribochemical reactions occurred when using BBST as lubricant additive.
Fig. 6 XPS of the wear scars on the test cylindrical with 10 wt% (a) BBST, (b) BOST, (c) MCCP, and (d) ZDDP in NBO. |
Fig. 6(b) shows the results of the Fe 2p, S 2p, N 1s, and O 1s spectra obtained from the XPS analysis when lubricated with 10 wt% of BOST in NBO. The Fe 2p peak observed at 710.2 and 723.6 eV corresponds to the FeS bond, which is consistent with the S2p peak observed at 161.4 and 163.7 eV, respectively.43 The 712.2 and 725.4 eV attributed to Fe2O3 and FeSO4 (combined with O 1s at 529.7 and 531.6 eV and S 2p at 168.1 eV).44 The N 1s peak appeared at 398.1 and 400.0 eV belongs to CN and Fe⋯N coordinate bonds.44 The present analysis assumes that the outstanding tribological performance of BBST and BOST in NBO is due to the generation of complex tribochemical products such as oxides, sulfide, and chemisorbed nitrogen compounds film during the tests.
The XPS analysis of the worn surfaces lubricated by MCCP shows the presence of iron(III) chloride (FeCl3) and iron(III) oxide-hydroxide (FeOOH) (Fig. 6(c)), whereas the ZDDP shows the presence of iron(III) phosphate (FePO4), FeS, poly(thio)-phosphate chains, non-bridging oxygen (NBO), bridging oxygen (BO), P–O–C bonds, P–O–P bonds, and Zn3(PO4)2 (Fig. 6(d)), respectively.30 The difference in the tribology performance of dimercaptobenzothiadiazole derivatives, MCCP, and ZDDP is attributed to the chemical composition on the tribofilm.4 The melting point of the FeS tribofilm (∼1193 °C) is higher than that of FeCl3 (∼306 °C) and FePO4 (∼250 °C) tribofilm. Consequently, the sulfur-based additives have higher weld preventing and protective film properties than that of chlorine- and phosphorus-based additives and thus gives excellent EP and AW performance.
Based on the EDX and XPS, it can be inferred that the π-electrons of the benzene ring and the lone pairs of N and S elements will electrostatically interact or physisorbed onto the iron surface. Subsequently, the N and S elements of the dimercaptobenzothiadiazole ring will undergo chemisorption with the metal surface to form a complex boundary film consisting of FeS, FeSO4, Fe2O3 and Fe⋯N coordinate bonds. This boundary lubrication film minimizes wear and prevents welding between the metal surfaces. It is presumably FeS and Fe2O3 are the main contributor to the excellent tribology performance due to their high melting point (>1193 °C).
Furthermore, the difference in the tribology performance of BBST and BOST is owing to the chemical structure. The MEPS displayed that the BBST has higher electron density in the overall structure due to the larger conjugated system from benzene ring to dimercaptobenzothiadiazole ring (Fig S6(a)†). Consequence, the π-electrons of the benzene ring in BBST could establish a non-covalent interaction with the vacant d-orbital of the iron surface to creates a donor–acceptor interaction that promotes the interactions between BBST and metal surface. The strong non-covalent interaction between the BBST and metal surface can create favorable conditions for the formation of coordination bonds, thus more S and N element from the dimercaptobenzothiadiazole can react with the metal surface to generate a metal salt tribofilm such as FeS, FeSO4, and Fe⋯N coordinate bonds. On the contrary, the hydrocarbon chains in BOST have less electron density as compared with BBST, and thus it has least interaction with the metal surface (Fig S6(b)†). Furthermore, the hydrocarbon chains in BOST may align horizontally to the metal surface, which will reduce and block other BOST molecules from adsorbing on the metal surface. Moreover, the BBST decomposes faster than BOST and thus allows more S and N active elements to adsorb on the metal surface and form a tribofilm. The EP and AW performance of BBST and BOST is in good agreement with their thermal stability. Therefore, both the S and N elements play a significant role in non-corrosive, AW, and EP performance. The adsorption of BBST and BOST on metal surface is illustrated in Fig. 7.
To examine the efficiency of the synthesized additives, we compare our additives with the previously reported additives which also use NBO as a base stock (Table 3). To the best of our knowledge, only three reports used NBO as base stock.30,49,50 Nano-TiO2 showed the lowest WSD at 0.07 wt%, which improved 1.03 times of wear reduction of the NBO.49 The addition of 0.1 wt% of graphite nanoflakes improved 2.5 times of wear reduction of the NBO but highly corrosive (corrosion grade 2c) to copper-based materials.50 Besides, our previous works30 found that the dioctyl disulfides and dibenzyl disulfides additives are non-corrosive and possess excellent EP and AW performance in the NBO. In this work, the dimercaptobenzothiadiazole-based additives, such as BBST are found to be ashless, non-corrosive, and exhibit excellent EP and AW performance compared to toxic conventional additives, such as MCCP and ZDDP. This indicated that BBST shows promising potential as an alternative EP and AW additives to replace MCCP and ZDDP. In general, NBO is a widely used base oil for industrial applications, such as insulating oil, compressor oil, and MWFs, etc29. Therefore, the exploration of the EP and AW additives in NBO is highly desired.
Entry | Additives | EP | AW (Wear reduction times) | Corrosion grade | Ref. | |
---|---|---|---|---|---|---|
PB (N) | PD (N) | |||||
1 | 0.07 wt% nano-TiO2 | — | — | 1.03 | 1a | 46 |
2 | 0.1 wt% graphite nanoflakes | — | 2.50 | 2c | 47 | |
3 | 10 wt% dioctyl disulfides | 1569 | 1961 | 4.63 | 1a | 30 |
4 | 10 wt% dibenzyl disulfides | 1961 | 2452 | 6.20 | 1a | 30 |
5 | 10 wt% MCCP | 1961 | 2452 | 5.29 | 1b | This work |
6 | 10 wt% ZDDP | 1236 | 1569 | 4.63 | 1b | This work |
7 | 10 wt% BOST | 1961 | 2452 | 4.63 | 1a | This work |
8 | 10 wt% BBST | 2452 | 3089 | 7.40 | 1a | This work |
(1) The synthesized dimercaptobenzothiadiazole derivatives, BBST and BOST consist of three sulfur atoms that are non-corrosive and ashless.
(2) The EP and AW of BBST are 3.13 and 7.40 times better than NBO at 10 wt%. The performance of BBST is also better than BOST, MCCP, and ZDDP.
(3) The outstanding tribology performances of BBST compared to BOST is due to the interaction of S, N, and π-electrons of benzene ring with the metal, and fast decomposition.
(4) BBST and BOST show great promise to replace commercial additives, such as MCCP and ZDDP.
(5) The formation of FeS and Fe2O3 under AW conditions provides excellent boundary lubrication films.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d3ra05692a |
This journal is © The Royal Society of Chemistry 2023 |