Tao
Rong
a,
Wei
Guan
a,
Weili
Song
b,
Haibin
Zuo
*a,
Jingxiu
Wang
a,
Qingguo
Xue
a and
Shuqiang
Jiao
*a
aState Key Laboratory of Advanced Metallurgy, University of Science and Technology Beijing, Beijing, 100083, China. E-mail: zuohaibin@ustb.edu.cn; sjiao@ustb.edu.cn
bInstitute of Advanced Structure Technology, Beijing Institute of Technology, Beijing, 100081, China
First published on 21st November 2022
Developing new precursors of synthetic graphite from harmful carbon-containing solid waste generated by coking enterprises has been an important topic in graphitization research for the world's green development and creating new energy. In this study, coke oven deposited carbon was used as a precursor to prepare graphite by a molten salt electrolysis method. The structure transformation law of deposited carbon and the changes of the O, N, and S atomic contents on the surface during the electrolysis process were explored. The results showed that deposited carbon is transformed into a graphitic structure with a graphitization degree of 0.74 and the conversion rate of O, N and S exceeds 50% in the molten CaCl2 salt under 2.6 V at 900 °C for 8 h. The low-temperature graphitization transition process of deposited carbon assisted by an electric field was investigated by molecular simulation calculations. Deposited carbon-derived graphite was demonstrated as a useful negative electrode material for lithium-ion batteries and delivered a high reversible capacity of 325 mA h g−1 and an excellent coulombic efficiency of 99.5% at 1C after 600 cycles, which could provide a reference for value-added utilization of carbon-containing solid waste in coking enterprises.
Currently, researchers attempt to prepare synthetic graphite from a variety of materials, including semi-coke,16 bituminous coal,12 waste PET plastic,13 poly vinyl alcohol17 and lignin.18 However, excellent precursors should be sustainable, inexpensive, and easily accessible. Due to the above characteristics, deposited carbon (DC) in coke ovens, which is a kind of coking by-product, has been paid more and more attention and studied as a potential precursor. DC is generated by the pyrolysis of crude gas in the coking process and commonly found in coking chambers and ascension pipes.19,20 DC that causes uneven temperature in the coking chamber and hinders coke pushing19 is harmful to coking production. The potential output of DC in coke ovens is relatively large, which is directly related to the operating system of coking enterprises. Taking the production data of a coking enterprise in China as a calculation reference,21 the potential production of DC in China and worldwide is about 1 million tons (Mt) per year and 1.5 Mt per year, respectively. It is worth noting that in China, the potential DC amount has even far exceeded the natural graphite production in 2017.22 However, there have been no efficient and valuable utilization methods available for treating DC.19,23 Therefore, it is of great significance to achieve the application of DC graphitization using DC as a precursor. Compared with other precursors, DC is not inferior in terms of chemical composition with a carbon content of not less than 90% and a low content of impurity elements in previous research.24,25 Hence, it is very important to perform further purification and utilization of DC. In addition, DC originates from coke oven emissions and contains polycyclic aromatic hydrocarbons, which seriously endanger the health of operators.26,27 Therefore, a harmless treatment of DC is urgently needed and DC can be a promising precursor for preparing graphite.
However, the current mainstream high-temperature (3000 °C) method to produce graphite is highly energy-intensive, and it has detrimental effects on the environment.15,28 Although the addition of various new and efficient catalysts can reduce the temperature of graphitization,29,30 the catalyst remaining in the graphite product generally limits the application of the catalytic graphite.30 In order to further reduce the processing energy consumption and the adverse effects of production methods, researchers have made many attempts for graphitization. Jin et al.31,32 brought surprises to other researchers by graphitizing carbon black at 800–950 °C through molten salt electrolysis and laid the foundation for graphitization transformation of solid carbon materials by molten salt electrolysis. Later, Zhu et al.33 prospectively studied the behavior of the oxygen element and the electrolytic graphitization process of hyper coal in molten CaCl2. The optimized electrolysis product was applied as an anode for lithium-ion batteries with a good electrochemical performance. Thapaliya et al.34,35 expanded the types of precursors and further verified the possibility of molten salt electrolysis graphitization by studying the graphitization transition behaviors of biomass-derived carbon and gasified coal chars under different electrolysis conditions. However, the carbon structure transformation law and graphitization mechanism of other carbon materials in the molten salt electrolysis process were not clearly presented, which were important guides for realizing the synergistic regulation of the structure and functions of carbon materials and further optimizing the process parameters, with the aim to achieve the application of carbon materials with low cost and high added value.
In order to achieve the high-value utilization of DC in coking enterprises, DC collected from ascension pipes in coking enterprises is used as a potential precursor to form a graphite based composite anode in this study. Through the method of molten salt electrolysis, DC was directly converted into flake graphite in molten salt at 900 °C for 8 h, when the cell voltage was 2.6 V. Molten salt low-temperature graphitization is more competitive in terms of energy consumption and production cost compared to the traditional Acheson process. The structure transformation law of DC and the mechanism of graphitization were explored, and the influence of the electric field on the molecular structure and electronic properties of the precursor was investigated. It was found that the electric field could affect electron injection and local charge redistribution during electrochemical graphitization. Graphitized electrolysis products were used in Li-ion batteries and the electrochemical performance was systematically evaluated in terms of reversible capacity and coulombic efficiency.
Anhydrous calcium chloride (AR, 96%) was purchased from Shanghai Macklin Biochemical Co., Ltd. Before the electrolysis experiments, it was dehydrated at a temperature of 300 °C according to a reported method37 to prevent the adverse effect of crystal water remaining in CaCl2 on electrolysis experiment.38
In order to verify the possibility of graphitization transformation of coke oven DC, the molten salt electrolysis process was conducted as shown in Fig. 1d. The electrolysis products shown in Table S2† were obtained under different electrolysis temperatures (850–950 °C), cell voltages (2.2–2.6 V) and electrolysis times (0–12 h). Through a variety of characterization methods, the effects of different experimental conditions on the structure of electrolysis products were investigated to clarify the mechanism of carbon structure transformation. In addition, the electrolysis products obtained under optimized conditions were used as electrodes in lithium-ion batteries to prove that DC-based electrolytic graphite can be used as an energy storage material.
XRD patterns were de-convoluted to reveal different carbon structures. Taking DC as an example (Fig. 2b), there are four curves in the range of 15–30° and 40–50° representing the γ band, 002 band, 100 band and 101 band.41,42 Then the structural parameters are calculated and listed in Table S3.† The degree of graphitization (G) is used as an important indicator to evaluate the graphitization transformation effect of DC in molten salt electrolysis. When the electrolysis temperature is 900 °C and the cell voltage is 2.6 V, the G value of the electrolysis product increases from −0.81 of DC to 0.74 of EP-12 h (Fig. 2c). It seems that the electrolysis time is positively correlated with the graphitization degree of the electrolysis product. The relationship between the G value and temperature is shown in Fig. S2.† The G value of EP-850 °C is only −1.06, which is even lower than the G value of DC. When the electrolysis temperature was raised to 900 °C, the G value of EP-8 h is greatly increased. The DC is transformed from an amorphous structure to a graphitic structure with an interlayer spacing of 0.3379 nm and stacking layer number of 51.40 (Fig. 2c). The electrolysis temperature can directly affect the viscosity of molten CaCl2,43 which affects the infiltration process of molten salt inside the working electrode. In a previous study, the graphitization of the carbon material did not occur when the carbon material was soaked in molten salt at 900 °C for 8 h.33 In this work, when the cell voltage was 2.2 V or 2.4 V, there was no graphitization of the carbon material. When the cell voltage was further increased to 2.6 V, the G value of EP-8 h was 0.74, suggesting that the cell voltage was the determining factor affecting the graphitization of DC in molten salt. Raman spectroscopy was widely used for studying subtle structural changes of carbon materials. As shown in Fig. 2d, it is obvious that the two peaks are the D peak at 1350 cm−1 and the G peak at 1580 cm−1 for all samples. The ratio of ID/IG is usually used as a criterion for determining the degree of structural ordering of carbon materials. Fig. 2e shows the ID/IG value of different samples. It was found that ID/IG values of EP-850 °C, EP-2.2 V and EP-2.4 V were higher than that of DC. This phenomenon could be caused by the condensation and polymerization of DC in the early stage of electrolysis. The breakage of chemical bonds in macromolecular compounds leads to the formation of defects and amorphous structures.44 According to the method reported,44–46 the Raman spectral bands ranging from 800 cm−1 to 2000 cm−1 were curve-fitted into five bands (D1, D2, D3, D4, and G). Raman spectral parameters such as peak position, full width at half maximum (FWHM), and intensity ratios were obtained (Table S4†). Fig. 2f shows the Raman spectrum of EP-8 h. The disappearance of the D3 and D4 bands means that the content of graphite carbon (sp2) increases significantly.46 Combined with XRD results, it is confirmed that EP-8 h was successfully transformed into a graphite structure. In Fig. 2g, ID1/IG decreases with the increase of electrolysis time, which suggests that the order degree of samples increases. ID1/IG of EP-12 h is 0.20 within the range of 0.11 to 0.30 as reported in the literature.32,33
In previous studies, sheet-like structures were prevalent in electrolysis products.31–33 However, in this study, SEM and TEM images of DC and electrolysis products also revealed the transformation of DC to a highly crystalline graphitic structure during molten salt electrolysis. Fig. 3a is a schematic diagram of the significant structural evolution of the DC surface during electrochemical graphitization. Specifically, as shown in Fig. 3b, the surface of the DC matrix is relatively flat, and there are some tiny spacings embedded in the substrate. These spacings may originate from natural growth during DC generation in coke ovens or from DC fragmentation prior to electrolysis.20 At the early stage of electrolysis, the surface of EP-4 h is densely wrinkled. These complex morphological changes are accompanied by the generation of local fractures in the samples, which was probably ascribed to the differences in the mechanical properties of different components under complex physical and chemical conditions. When the electrolysis time was further extended to 8 h, some obvious small-sized flakes appeared due to the structural breakage, and the pores were caused by irregular distribution of these flakes. These seem to be related to the stress release of the wrinkles in EP-4 h. It is noted that the individual flake appears to be flat at the micrometer scale. Obviously, the flakes are further enlarged to form flake clusters in EP-12 h compared with EP-8 h. It is concluded from both the XRD and Raman results that the key feature for the formation of the graphitic structure during electrochemical conversion is the appearance of flakes in EP-8 h and EP-12 h. The TEM image of the flakes in EP-8 h is shown in Fig. 3c. The high-resolution TEM image of EP-8 h (Fig. 3d) shows that the interlayer spacing is 0.3391 nm which is close to the value for natural graphite.47 Although the interlayer spacing of the petaloid flakes reported in our former study (0.3285 nm) is smaller than the flake structure in EP-8 h,33 EP-8 h appears to be competitive due to its high degree of graphitization and short production time. During the electrochemical transformation, the change of the sample microstructure affects its specific surface area and pore size distribution. Fig. 3e shows the N2 adsorption–desorption curves of DC and EP-8 h at −195.8 °C. The correspondingly calculated BET surface areas are 4.1161 m2 g−1 and 7.4926 m2 g−1, respectively. The lower surface area of amorphous carbon than graphite seems to be related to the difference in their structural unit size. After molten salt electrolysis, the specific surface area and the average pore size of the sample increased significantly. Fig. S3† shows the pore size distribution of DC and EP-8 h. The average adsorption pore size of the latter is much larger than that of the former (43.86969 nm vs. 16.64374 nm).
Fig. 4a shows the FTIR spectra of DC, EP-4 h, EP-8 h and EP-12 h at 1000–1800 cm−1. The absorption band located near 1100 cm−1 is caused by the stretching vibration of SO (1080–1120 cm−1) bonds and C–O–C (1120–1160 cm−1) bonds,48 and the broad absorption band around 1620 cm−1 is assigned to the stretching vibration of CC bonds in the aromatic structure.49 The intensity of the absorption peak is related to the amount of chemical bonds in the sample. Previous studies32,35 have shown that the electrolytic graphitization process of molten salts is accompanied by the occurrence of deoxidation reactions. As shown in Fig. 4b, the relative intensities (SO/CC and C–O–C/CC) decreased with the extension of electrolysis time in the current study. It can be speculated that the content of oxygen-containing chemical bonds in the DC decreased with the prolongation of electrolysis time. In Fig. 4c, the absorption bands in the wavenumber range of 2800–3000 cm−1 are ascribed to the stretching vibrations of aliphatic structures.50 Four peaks can be fitted including antisymmetric CH3 stretching, antisymmetric CH2 stretching, symmetric CH3 stretching and symmetric CH2 stretching.51 In the study of carbon materials, the aliphatic structural parameter A(CH2)/A(CH3) can be used to characterize the length of aliphatic chains and the degree of branching aliphatic side-chains.42,46,51,52 It can be calculated from eqn (1), where A2920 and A2960 represent the area of –CH2 and –CH3 groups, respectively.
(1) |
As shown in Fig. 4d, A(CH2)/A(CH3) decreases with the increase of electrolysis time, which implies that the aliphatic chains of the aromatics ring are gradually shortened and structures between aromatic rings become more compact in DC during the electrochemical conversion of molten salt.
XPS is the most sensitive method for probing the surface of carbon materials.53 The XPS spectra (Fig. 4e) show the presence of carbon, oxygen, sulfur and nitrogen in DC, EP-4 h, EP-8 h and EP-12 h. With the progress of the electrochemical conversion of DC in molten salt, the atomic contents of elements such as O, N, and S in the surface layer of the electrolysis product decrease with the increase in electrolysis time as shown in Table S5† and Fig. 4f.
Atomic conversion rate (R) was defined to represent the degree of removal of oxygen, nitrogen and sulfur atoms on the surface of DC during the electrochemical conversion in molten salts. It can be calculated using eqn (2), where X represent atomic species, including O, N and S; A[X],0 represents the atomic percentage of X in DC, %; A[X],t represents the atomic percentage of X in products prepared after electrolysis for t h, %.
(2) |
Under the current electrolysis conditions, the atomic conversion rate of N atoms on the surface of DC is highest after 12 h of electrolysis (Fig. S5†). Normalizing the data in Fig. S5,† the atomic conversion rate of S atoms on the surface of DC is smallest in the range of 8–12 h as shown in Fig. S6,† which indicates the complete removal of S atoms, but the removal process of O and N atoms is in progress.
The removal of O, N, and S during electrolysis is accompanied by the evolution of the chemical structure of C in DC. Fig. 4g shows the high resolution XPS spectra of C 1s for DC and EP-8 h, and the deconvolution of the C 1s peaks showed 3 different peaks: sp2, sp3 and π–π* shake-up feature.54 The sp2 represents carbon in CC bonds in aromatic rings and in aliphatic chains,53 sp3 represents carbon in CH2 and CH3 (ref. 54) and π–π* transitions are common in aromatic ring structures.55 Table S6† shows the results of chemical bonds calculated from XPS measurements. Fig. 4h shows the relative area of sp2 and sp3 in DC, EP-4 h, EP-8 h and EP-12 h. With the increase of electrolysis time, the content of graphite carbon (sp2) in the DC increases. In summary, the curve of relationship between the working current and time is shown in Fig. 4i. In the early stage of electrolysis, a large current response is associated with double layer charging.31 Then, the current quickly drops to below 0.45 A. In this study, the O, N, and S atoms in DC were gradually removed, with the S atom being first stabilized. During the electrolysis process, the disordered C atoms in DC are subsequently rearranged with a long distance, and stacked into a highly ordered graphitic structure. The current response stabilizes at about 0.15 A at the later stage of electrolysis.
The energy efficiency (e) of the molten salt process is specified in eqn (3).
(3) |
More and more studies56–59 have shown that the electric field could cause a series of physical and chemical changes in materials, affecting the molecular structure and electronic properties of materials. In order to explore the effect of electric field on the molecular structure of DC during molten salt electrolysis, DC was simplified into a structure with seven benzene rings attached to one functional group. At room temperature, the experimental structure with –CH2CH3 was optimized as shown in Fig. 5a. When electric fields of different strengths (0, 0.001 eV Å−1 e−1 and 0.01 eV Å−1 e−1) were applied in the X-axis direction, the bond lengths d1 and d2 in the –CH2CH3 structure increase with the increase of the electric field (Fig. 5b and c), and the bond angle ∠A decreases with increasing electric field (Fig. 5d). In the absence of an applied electric field, the degree of ordering of the precursors immersed in molten salt shows almost no variation.33 After the application of an electric field, the stable molecular structure of the DC accelerates the transformation to a highly ordered structure under the action of the electric field force. Furthermore, as shown in Fig. 5e, the electric field significantly affects the local charge density in the molecular structure. The charge density of a specific structure correlates with the catalytic activity,60 specifically, the reactivity of functional groups containing O, N, and S. Due to the occurrence of deoxidation, denitrification, and desulfurization reactions of DC, it is concluded that the changes of the charge density of a specific structure are related to electrochemical graphitization.
DC contains various elements such as S, C, and O, implying the presence of various functional groups, including –COOH, –CHO, –OH, –NH2, –SH, etc. During molten salt electrolysis, the electric field changes the number of the charge population of O, N, and S atoms in functional groups (Fig. 5f). The electronegativity of atoms in the local molecular structure can be changed under the electric field,61,62 which represents the electron attracting ability of functional groups containing O, N, and S, and affects the transfer of electrons between atoms.
In this study, it was found that the electric field accelerates the transformation of DC to the graphitic structure, affects electron injection and local charge redistribution and promotes the deoxidation, denitrification, and desulfurization reactions of DC during electrochemical graphitization.
Fig. 6a shows the CV curves of EP-8 h. In the first cycle, there was an obvious wide reduction peak at 0.7 V but it disappeared in the second and third cycles, which is related to the generation of irreversible SEI films.14,63 This phenomenon also occurs in other investigated electrolytic carbon materials, such as biochar-based electrolytic graphite34 and coal char-based electrolytic graphite.35 In addition, the reduction peak near 0.1 V represents the process of lithium ion intercalation into graphite, and the oxidation peak at 0.3 V represents the process of lithium ion extraction from graphite.14
The initial discharge capacity of EP-8 h is 452 mA h g−1 at 1C as shown in Fig. 6b, which is significantly higher than that of commercial graphite (313 mA h g−1). Besides, the reversible capacities in the second cycle of electrolytic carbon and commercial graphite are almost the same. The initial irreversible capacity and initial coulombic efficiency of EP-8 h are 154 mA h g−1 and 65%, respectively. The initial irreversible capacity of EP-8 h is related to the formation of dead Li and a stable SEI.64 After molten salt electrolysis, the specific surface area of DC increases and the mesoporous structure is more developed, which can provide more intercalation sites for lithium ions and cause soft short circuits and severe dendrite formation, resulting in capacity attenuation.64
At the rates of 0.1C, 0.2C, 0.5C and 1C, the average discharge capacities of EP-8 h are 302.62 mA h g−1, 297.11 mA h g−1, 289.60 mA h g−1 and 279.09 mA h g−1 (Fig. 6c), and when the current density was restored to 0.2C, the capacity of DC could still be maintained at 295.41 mA h g−1 (average capacity of 20 cycles), similar to the commercial graphite reported in the literature.65 This demonstrated that the electrolytic graphite produced by low-temperature graphitization exhibits a good rate capability due to the complex flake structure and prepared mesoporous structure.
Fig. 6d shows the good long-term cycling stability of EP-8 h at 1C. After 600 cycles, EP-8 h can still maintain a high reversible capacity of 325 mA h g−1 and an excellent coulombic efficiency of 99.5%. During cycling, the specific capacity of EP-8 h increases slightly, which is related to the activation of lithium ions and is a common performance of porous carbon-based materials.66
The reversible capacity and coulombic efficiency are important indicators for evaluating the electrochemical performance of batteries.64 In previous studies, activated coconut (ACC),34 gasified coal char (GCC),35 hyper coal (HPC)33 and amorphous hard carbon (HC)67 were converted into graphite materials by molten salt electrolysis, and the optimized electrolysis products were applied in lithium-ion batteries. Comparing EP-8 h with these precursors, the electrolysis products based on DC exhibit a good performance with a stable reversible capacity and a common initial coulombic efficiency (Fig. 6e), which illustrates the promising application prospect of DC-based electrolytic graphite materials in lithium-ion batteries.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ta08198a |
This journal is © The Royal Society of Chemistry 2023 |