Marcin W.
Orzech
a,
Francesco
Mazzali
a,
Arturas
Adomkevicius
a,
Mauro
Coduri
b,
Yubiao
Niu
c,
James D.
McGettrick
c,
Philip A.
Chater
d,
Laura
Cabo-Fernandez
e,
Laurence J.
Hardwick
e,
Lorenzo
Malavasi
b and
Serena
Margadonna
*a
aFuture Manufacturing Research Institute, College of Engineering, Swansea University, Swansea, SA1 8EN, UK. E-mail: S.Margadonna@swansea.ac.uk
bDepartment of Chemistry and INSTM, University of Pavia, 27100 Pavia, Italy
cAIM and SPECIFIC, College of Engineering, Swansea University, Swansea, SA1 8EN, UK
dDiamond Light Source Ltd, Diamond House, Harwell Science and Innovation Campus, OX11 DE Didcot, UK
eStephenson Institute for Renewable Energy, Department of Chemistry, University of Liverpool, L69 7ZD, Liverpool, UK
First published on 6th September 2024
Sodium-ion batteries represent a sustainable and cost-effective solution for grid-scale energy storage. However, the reliance on cathode materials containing scarce transition metals currently limits their wider adoption. Carbonaceous materials present an environmentally sustainable and economically viable alternative. This study investigates the application of reduced graphene oxide as a cathode active material. A detailed analysis of the storage mechanism and its dependence on the morphological and chemical structure revealed that it combines surface capacitance and faradaic reactions. The key factors responsible for high capacity and long cycle life are the open structure of graphene sheets and the presence of functional oxygen and nitrogen groups where Na+ ions are stored in the R–CO + Na+ + e− ↔ R–C–O–Na reaction. A good understanding of the mechanism allowed optimisation of cycling conditions in a proof-of-concept all-carbon full cell incorporating reduced graphene oxide and hard carbon as a cathode and an anode, respectively. The system displays good energy density (80 W h kg−1) and remarkable stability over 500 cycles. The gained insights will support the rational design of more efficient carbonaceous electrodes.
The most studied electrode materials for SIBs are hard carbons as anode active materials and a few groups of cathodes: transition metal oxides, polyanions, and Prussian Blue analogues. Hard carbons are an effective and sustainable substitution for expensive graphite used in LIBs.6–9 On the other hand, the cathodes often contain transition metals (including cobalt) presenting the same concerns and limitations in terms of cost and sustainability as those currently employed for LIBs. Furthermore, most of the intercalation compound cathodes, also considering phosphates and fluorides, suffer from either low sodium storage capacity and rate capability or poor cycle life.10,11
A promising solution to sustainability and cost concerns as well as performance limitations is the use of carbon as the active material for both electrodes.12 Carbonaceous materials are inexpensive, environmentally friendly and highly conductive. Recent works on the utilization of organic or carbonaceous materials as cathodes for LIBs, such as aromatic carbonyl derivative polymers,13 functionalised carbon nanotubes (CNTs)14,15 and reduced graphene oxide (rGO)16–20 showed promise for ‘green’ and sustainable batteries. Nevertheless, research on applying this approach in Na-ion batteries is still lagging behind and focuses mostly on the negative electrode side.21
Recently, Ali et al. reported on the electrochemical performance of rGO as a suitable cathode for SIBs.22 It showed a high specific capacity of 235 mA h g−1 and stable behaviour over 1000 cycles. The authors ascribed the outstanding performance to pseudocapacitive storage and reversible sodium adsorption on graphene layers, which benefits from the high surface area of the material. Notably, it was the first time that rGO was used as the only active material for the Na-ion cathode, instead of as an additive that enhances the performance of the electrode.21,23–25 Another work on hollow graphene nanospheres demonstrated that the surface mechanism of Na+ ion reactions with functional groups improved the specific capacity of the cathode and allowed stable cycling at very high current rates of up to 40 A g−1.26 The reported mechanism is similar to reversible redox reactions with oxygenic functional groups observed in functionalised carbon electrodes for LIBs.27–31 The most commonly reported energy storage mechanisms observed in carbonaceous cathodes are either intercalation in dual-ion type cells32–35 or electrical double-layer capacitive (EDLC) storage in supercapacitors.36 However, reports on rGO more often point to a combination of pseudocapacitive behaviour and surface redox reactions with functional groups.37–39 The fundamental understanding of these mechanisms is still lacking, which hinders the rational design of carbonaceous cathode materials.
This work investigates the underlying mechanism in detail and applies the gained knowledge to construct an all-carbon full cell with excellent stability. Two reduced graphene oxide cathodes, differing in morphology and chemical structure, were investigated for their potential use in SIBs. The primary energy storage mechanism in both cases was found to be absorption. However, by the use of in situ Raman spectroscopy and X-ray pair distribution function (PDF), additional processes were identified that contribute to good performance. They involved surface faradaic reactions between the sodium ions and the functional groups as well as the bipolar behaviour of rGO resulting in additional capacitive storage of ClO4− anions. This discovered hybrid energy storage mechanism results in a significantly increased gravimetric capacity. A proof-of-concept all-carbon full cell with rGO as the cathode and hard carbon (HC) as the anode, showed a specific energy of 80 W h kg−1 and high stability over 500 cycles, confirming that rGO is a viable cathode material for SIBs. These findings support the way to the design and development of more sustainable energy storage systems.
For the in situ X-ray pair distribution function (PDF) measurements, the same free standing electrodes were used. The in-house made Swagelok-type cells provided by beamline were assembled with Na metal counter electrode and a glass-fibre separator (Whatman, GF/D). In the used radial geometry, it is possible to slice just through the electrode of choice and get data from electrodes as thin as 50 microns. The cells were cycled galvanostatically at a rate of C/10 in the range of 1.0 to 4.5 V. X-ray total scattering data were collected with an exposure time of 120 s. Data were collected for the first sodiation, the first desodiation, and the second sodiation. X-ray scattering data were collected at the I15-1 beamline at the diamond light source using an X-ray energy of 76.7 keV (λ = 0.1617 Å) and a flat panel detector (CeO2 standard). The experimental 2D raw images were automatically reduced at the beamline. All scattering contributions but the signal coming from the rGO cathode, such as empty cell, electrolyte and separator were subtracted. PDFs were computed using the PDFgetX3 software.42 Data were truncated to Qmax = 24 Å−1 before Fourier Transform.
Investigations of the chemical composition and structure of the two samples were performed through X-ray photoemission spectroscopy (XPS). The high resolution C1s, N1s and O1s (Fig. 1(D)–(I)) spectra were recorded to highlight the presence of different oxygen and nitrogen containing functional groups. The C1s spectra show a very similar distribution between sp2 (CC) and sp3 (C–C) hybridization. On the other hand, the oxygen and nitrogen contents vary between samples, reflecting a difference in the functional groups. The O/C ratios are 0.15 and 0.13 for rGO_1 and rGO_2, respectively, which shows that after reduction more oxygenic functional groups remained in the former. However, to get a better idea on the total content of functional groups also nitrogen should be considered. The O + N/C ratios are 0.16 and 0.17 for rGO_1 and rGO_2, respectively, which reveals that the latter is slightly more functionalised. Comparing the fitted envelopes, it can be inferred that rGO_2 contains less epoxide (C–O–C) and carboxyl (HO–CO) groups, but a higher amount of carbonyl (CO) functional groups than rGO_1. The amount of hydroxyl (C–OH) groups is comparable in both materials. The two samples present a clear difference in nitrogen content −0.6% and 3.3% for rGO_1 and rGO_2, respectively. The only nitrogen bonds detected in the former were pyrrolic N, while in rGO_2, all three – pyridinic, pyrrolic and graphitic–nitrogen bonds were present, with pyrrolic N (1.5%) and pyridinic N (1.2%) dominating. It has been reported that the introduction of N atoms, particularly pyrrolic and pyridinic, causes more edges as well as open and flexible vacancy defects for increased reversible Li+ and Na+ ions storage in graphene cathodes.37,44,45
Raman spectroscopy is one of the most insightful techniques for characterisation of carbonaceous materials. The Raman spectra of both samples were recorded at an excitation wavelength of 532 nm (Fig. 1(B) and (C)). They demonstrate the typical fingerprint of D (∼1350 cm−1) and G (∼1590 cm−1) bands found in sp2 carbons. Spectra were fitted with 5 peaks, in analogy with previous work.46,47 Besides D and G, the other three peaks are D′, A and D* (Table S2, ESI†). The D′ feature is another E2g graphitic lattice mode and has been attributed to disorder in a surface layer, i.e. graphene layers which are not directly sandwiched between two other graphene layers.48,49 The ID′/IG ratio has been assigned to the intercalation between carbon layers50 or covalent bonding on the surface of the CNTs.51 The A band is located around 1500 cm−1 and corresponds to amorphous carbon;46,47,49 furthermore Claramunt et al. correlated the inversely proportional relation of IA/IG and FWHM of the A band to the crystallinity of rGO.47 The D* band is located between 1100 and 1200 cm−1 and is related to an additional defect mode provided by sp2–sp3 bonds at the edges of networks.52 Particularly, the ID*/IG ratio increase corresponds to an increase in the number of sp3 bonds at the edges of graphene sheets.47
The data derived from fitting the Raman spectra of the raw powders are summarised in Table S2 (see the ESI†). The relative intensity ratio of the main peaks (ID/IG) can be used to estimate the defect concentration.53,54 Slightly higher value of the ID/IG ratio in rGO_2 (1.50) compared to rGO_1 (1.45), and broader D band suggests more a disordered nature of the rGO_2 sample, which is in agreement with the XRD and the higher O + N/C ratio derived from XPS measurements. The defects on the graphitic surface layers are indicated by the ID′/IG ratio, which is higher for rGO_1 (0.40) compared to 0.33 for rGO_2 (0.33). The XPS results suggest that this difference comes from more epoxy functional groups in rGO_1, which develop at the basal plane of the graphene sheets creating the in-plane defects and disorder.55,56 Very close values of IA/IG and ID*/IG reveal similar crystallinity and concentration of edge bonds in both samples.
The morphologies of the two materials were studied using electron microscopy (Fig. 2). From the SEM images, it can be clearly seen that rGO_2 (Fig. 2(D)) adopts the form of large flakes sized 0.1–1 μm comprising ultra-thin graphene oxide sheets (<1 nm). Large channels and voids formed by the sheets are clearly visible and creating an interconnected 3D porous network. Instead, rGO_1 (Fig. 2(A)) presents a bulkier morphology with particles that are a few micrometres in size. Thin graphene layers are clearly observed; however, they are agglomerated into closed structures. These morphological differences are significant, as rGO_2's large, thin flakes and porous network contrast sharply with rGO_1's bulkier and more agglomerated structure. This distinction is crucial for applications requiring high surface area and efficient electrolyte penetration. The more open and dispersed structure is additionally confirmed by the higher specific surface area (BET) of rGO_2 (865 ± 29 m2 g−1) than rGO_1 (461 ± 38 m2 g−1). For comparison, the reduced graphene oxide studied by Ali et al.22 had a specific surface area of 789 m2 g−1. The high specific surface area and porous interconnected network are generally considered beneficial for short ion diffusion paths. Fig. 2(C) and (F) show the high-angle annular dark-field (HAADF) scanning transmission electron microscope (STEM) images and the corresponding energy-dispersive X-ray spectroscopy (EDX) line scans of rGO_1 and rGO_2, respectively. The rGO_2 flake in Fig. 2(E) is extensively creased, which creates many inner voids, while the rGO_1 flake presented in Fig. 2(B) has a smoother morphology. The EDX line profiles confirmed the presence of functional groups in both samples. The total content of oxygen and nitrogen was higher in rGO_2 (14.3%) than in rGO_1 (7.9%). Although the EDX measurements of such light elements have a low quantitative value, the trend of more functional groups in rGO_2 is in good agreement with more accurate XPS results.
It is known that careful choice of the binder used in electrode fabrication can greatly influence the electrochemical performance upon cycling, owing to its ability to maintain structural integrity upon volume changes and negligible interactions with the electrolyte.57–59 The PVDF binder is commonly used in LIB cathodes, yet for sodium chemistries, CMC is emerging as the binder of choice thanks to its low toxicity and high stability in sodium electrolytes.60 Another rGO_2 electrode was therefore prepared with CMC instead of the PVDF binder, with the aim of maintaining its high capacity and extending cycle life. Cycling results (Fig. 3(A)) show that the stability of the electrode was noticeably improved. Indeed, no capacity fading was observed in the first 50 cycles retaining 241 mA h g−1. Moreover, the average Coulombic efficiency was as high as 98.7% indicating enhanced reversibility. Nonetheless, the capacity started to diminish rapidly after 50 cycles, resulting in less-than-ideal overall performance, which might suggest the presence of some degradation mechanism.
Rate capabilities of both cathodes were studied at 30, 60, 150, 300, 600 and 1500 mA g−1 current densities (Fig. 3(C)). The rGO_2/CMC maintained the high capacity of 117 mA h g−1 at 1500 mA g−1. On the other hand, the rGO_1 based electrode achieved 76 mA h g−1 at the same current rate. In all cases, the electrodes retained ∼50% of the initial capacity at the highest current rate. Notably, both rGO_2/PVDF and rGO_2/CMC achieved higher capacities at 600 mA g−1 (respectively, 136 and 146 mA h g−1) when compared with previous work.61 Both materials restored the initial capacity after returning to 30 mA g−1, indicating good stability at a high discharge current. However, capacity fading upon prolonged cycling remains an obstacle on the road to the practical utilization of high energy and power capabilities of the rGO cathode; thus, the energy storage mechanism has to be understood to find the root cause.
The first five charge and discharge potential profiles of both cathodes with PVDF binder exhibit smooth curves without obvious plateaus (Fig. S2, ESI†), characteristic of typical EDLC behaviour,62 in agreement with previous results.61 This indicates that the storage mechanism is predominantly based on non-diffusion limited surface reactions, in line with the observed good stability at high current rates. This is reflected in the higher capacity of rGO_2, which has more open and exposed graphene flakes with a higher specific surface area, facilitating better electrolyte penetration and more accessible surfaces compared to the compact rGO_1 particles.
The potential derivatives of the specific capacity curve (dQ/dV vs. V) plots give more detailed insights into the electrochemical behaviour (Fig. 3(B) and (D)). During the first charge, a significant increase in oxidation current is observed above 4.2 V, which diminishes in subsequent cycles, indicating irreversible reactions.61 It was reported that NaClO4-based electrolytes can undergo decomposition at very high potentials vs. Na/Na+ due to the oxidizing nature of ClO4− anions.63–65 Additionally, nitrogen atoms lower the energy barrier and can catalyse ClO4− degradation.66,67 The effect of nitrogen-induced electrolyte oxidation above 4.2 V was also observed in the mesoporous graphene cathode for Na-ions.37 These results point toward a scenario where above 4.2 V, irreversible oxidation of the electrolyte limits the cycle life of the cell, a phenomenon that is more pronounced in the rGO_2 electrode, which has a higher nitrogen content.
In subsequent cycles, the dQ/dV curves of both rGO samples show small, broad features between 2.2 V and 3.5 V on charge and at 2.9 V on discharge, indicating reversible redox reactions. The rGO_2 cathode also displayed an unusual dQ/dV feature at 1.3 V on the discharge curve, potentially due to contamination from H2O produced during perchlorate anion reduction.68–70
Notably, replacing the PVDF binder with CMC did not affect the potential curve shapes (Fig. S4, ESI†). To better understand the origin of the faradaic components, the reactions occurring upon cycling and the causes of capacity degradation, the sodium storage mechanism in rGO cathodes was further studied using in situ Raman spectroscopy and in situ X-ray PDF measurements.
In the reverse scan (desodiation), a major blue shift (Δ = 12 cm−1) and a sharpening of the G band (Δ = −8 cm−1) are observed. This change is linear in the whole potential window. The G band returns to the position observed at OCV at around 3.5 V, which corresponds to the switch from the n-doped state back to the neutral state. Above 3.5 V, the changes continue in the same manner. The frequency shift and sharpening of the G band have been linked to the changes in the Fermi surface of graphene due to the p-doping effect.77,81 In the functionalised rGO and organic electrodes, the reversible association and dissociation of electrolyte anions (ClO4− or PF6−) on the material's surface above 3.0 V vs. Li/Li+ (2.7 V vs. Na/Na+) was reported.20,82–84 This leads to charge transfer and the formation of the [(RN)+xAx−] complex, for example [(N)+x (PF6−)x],83 causing the creation of the p-doped state of reduced graphene oxide. Hence, the oxidative current increase above 3.5 V, correlated with the significant blue shift and sharpening of the G band in the Raman spectra of rGO_2, is at least partly associated with p-doping from ClO4− anions association. However, the presence of NaCl in the electrode indicates that the part of the charge reaction above 4.2 V is related to the irreversible electrolyte decomposition.68 The ClO4− reduction can additionally be catalysed by the presence of nitrogen atoms.67,85–87
Nevertheless, in the second discharge, no G band changes down to 3.5 V were observed. This indicates that the negative charge from ClO− maintained the p-doped state of rGO. Starting from 3.5 V, a red shift of the G band was detected, which demonstrates the disassociation of ClO− anions, i.e. the reversal of the p-doping. Additionally, the largest change in the G band position occurs between 3.0 V and 2.5 V, which is correlated with a reduction peak at 2.9 V. Recent studies on functionalised rGO, GO or CNT electrodes for LIBs reported on reversible reduction and oxidation of oxygenic functional groups in reaction CO + Li+ + e− ↔ C–O–Li.13–17,82,88,89 Therefore, the 2.9 V reduction peak and the corresponding downshift of the G band can be attributed to the Na+ redox reaction with the oxygen functional groups on the reduced graphene oxide surface: CO + Na+ + e− ↔ C–O–Na.14,20,83,88 At 1.2 V, the G band position is the same as in the first discharge, confirming the reversible formation of the n-doped state. Similarly, for the second charge, the G band blue shift is repeated, as well as the oxidation peaks at 2.7 V and 3.25 V, indicating that the redox reaction with functional groups and the p-doping of rGO are reversible.
The in situ Raman measurement rGO_1 sample was conducted as well, and the spectra of the first two discharge/charge cycles showed a similar pattern to rGO_2. For a detailed study and comparison, the spectra of both samples at OCV and cut-off potentials were fitted with 5 peaks as described earlier (Fig. 4(C) and Fig. S5, ESI†). Fig. 5 shows key Raman parameters plotted versus cell potential. It was observed that the G peak component of the G band (Fig. S6A, ESI†) shifts to a lower wavenumber on discharge. Interestingly, initially in the rGO_2 electrode, the G peak was located at a higher wavenumber due to the nitrogen content; however, at 1.2 V, it is the same (1585 cm−1) for both samples. This indicates that the influence of the N lone-pair electrons on phonon dispersion is neutralised and Na–N bonds are formed, which increases rGO_2 capacity analogously to Li-ion systems.83 When the cells were charged to 4.5 V, the G peak returned to the frequency just below the OCV position. Therefore, the apparent major blue shift of the G band described above is in fact caused by the increase in the D′ peak intensity (red colour in Fig. S6A, ESI†). The increase in the ID′/IG ratio during the oxidation scan is ascribed to the release of Na+ and consequent oxidation of epoxy functional groups15 followed by ClO4− anions association on the surface of rGO and p-doping. Additionally, the changes in the FWHM of the G peak (Fig. S6B, ESI†) in the rGO_2 sample confirm the p-doping – i.e. stiffening at 4.5 V was observed. This effect was less obvious in rGO_1 due to the lower nitrogen content and the absence of pyridinic groups.83 In the second discharge, the ID′/IG ratio and FWHM returned to previous values, indicating that this mechanism is reversible.
The defect concentration in the carbon materials is mainly associated with the D/G peaks intensity ratio (Fig. S6A, ESI†). During the CV scan of both samples, the ID/IG ratio is very close and changes accordingly with sodium de/insertion. It increases with discharge and decreases with charge. Additionally, a corresponding increase and decrease in the FWHM of the D peak is observed (Fig. S6B, ESI†). This suggests that sodium intake increases the defect concentration in rGO, while its release has the reverse effect. This is also reflected in the IA/IG ratio (Fig. S6C, ESI†) linked to the amorphous portion of the rGO, which increases at 1.2 V and drops at 4.5 V. The ID*/IG ratio (Fig. S6C, ESI†) is associated with the sp2–sp3 bonds at the edges of graphene layers. In the first discharge of both samples, at 1.2 V, the intensity of the D* peak is significantly reduced, while in the subsequent charge, reverse change is observed. This behaviour indicates the storage of Na+ ions at the edges of graphene layers.19 Moreover, the ID*/IG ratio at 4.5 V is close to its value at OCV, suggesting that ClO4− anions associate rather at the basal plane of rGO, contrary to Na+ storage at the edges. The decrease appeared again in the second discharge, confirming the reversibility of the process.
To gain further insights into the storage mechanism, in situ X-ray total scattering measurements were performed to study real-time local structural changes during cycling. As no significant difference between rGO_1 and rGO_2 was observed, only the latter was analysed in detail. The experimental patterns (Fig. S7, ESI†) collected in situ at different potentials, corresponding to maximum sodiation and desodiation, reveal no signification variation. This indicates that there are no significant structure changes in the bulk of rGO during cycling. Similarly, the corresponding PDF data reported in Fig. 5(A), obtained from the Fourier transform of the corrected and normalized total scattering data, show no changes with the peak positions remaining constant within 0.01 Å.
The experimental PDF shows only three well-defined peaks, indicating the absence of long-range order, in agreement with the diffraction data. The first peak occurs at 1.4 Å, which is consistent with the tabulated C–C bond length for graphene (1.42 Å). No evidence of the C–O bond is observed because of their low frequency and the similarity with the C–C distances. The PDF intensity is generally averaged over all atom pairs, and therefore the observed signal is dominated by C–C correlations of the graphene skeleton. In order to understand the origin of the other two peaks located at 2.4 Å and 3.7 Å a graphene layer should be considered. Even though experimental PDF studies on graphene are scarce, examples of calculated PDF are given in the work of Kumar et al.90 and these are obtained by considering a model where every C atom lies at the intersection of three C6 hexagons (Fig. 5(B)). Centring on this C atom and assuming a flat layer, one can draw circles intercepting the next C atoms and each circle corresponds to an interatomic distance, i.e. a positive correlation in the PDF. The second peak corresponds to the 2nd and 3rd neighbours within a hexagon. As the peak at 2.8 Å has a lower multiplicity, it is hidden in the background. According to this model, the presence of a clear peak in the experimental PDF at 2.4 Å indicates a coherent region composed of 3 hexagons. The third PDF peak is broader with lower intensity and even broader features are observed at larger interatomic distances. These should correspond to the centre of mass of nearby C6 hexagons, not arranged coherently because of the presence of defects. The results indicate that atomic structure is well ordered only within a few hexagons while the layer is disordered, or corrugated, so that rigid correlation between far hexagons is lost. As no changes are observed in the PDF data when the rGO cathodes were cycled in the full potential widow, it follows that the structural disorder induced by the sodiation/desodiation process is negligible compared to that already present in the pristine samples. Furthermore, the obtained PDF data do not show changes in peak position or width upon cycling, implying that interlayer expansion and contraction occurring during discharge and charge can be ruled out. This infers the absence of an intercalating behaviour and the lack of charge transfer between sodium and the p-band of the graphene sheet.
The detailed analysis presented describes a scenario where the storage mechanism of rGO as a cathode is pseudocapacitive-like, predominantly based on the absorption of ions on the surface of the graphene-like sheets. The more open and exposed morphology of rGO_2 flakes compared to the closed and compact particles of rGO_1 supports more extensive electrolyte penetration and more sites for ion storage, resulting in a higher specific capacity.91 However, other reactions also take place, playing a major role in determining the electrochemical performance, contributing to the total capacity as well as defining the long-term cycling stability. Particularly, the faradaic mechanism can be divided into two stages. First, below 3.5 V, the Na+ ions are stored at the defects and edges of rGO and through redox reaction with the O and N functional groups. Then, above 3.5 V, the association of anions from the electrolyte on the rGO basal plane occurs. These processes are seen in the in situ Raman as a continuous and linear transition from the p-doped state (oxidised state) to the n-doped state (reduced state). However, these are not observable in the PDF data as they apply to a fraction of the material and do not induce structural changes in the bulk. In the rGO_2 electrode, the nitrogen content improves the specific capacity, owing to coordination interaction between Na and N lone-pair electrons (Na–N bonding)83 as well as increased absorption of ClO4− anions near N-functional groups.67,85 However, the heteroatoms also act as catalysts for electrolyte degradation above 4.2 V, causing capacity fade. The capacity loss is smaller in the rGO_1 due to lower nitrogen content, but the effect on cycle life is still rather significant.
It is worth noting that a similar mechanism of utilisation electrolyte salt anions as charge carriers has been applied in so-called ‘dual ion’ batteries.92 However, in this case, the anions are stored in a graphite cathode via an intercalation mechanism, which delivers relatively low capacities. For instance, Fan et al. reported on soft carbon-graphite Na-ion ‘dual carbon’ cell, where graphite cathode delivered a small capacity of around 40 mA h g−1,93 or in another example, the graphitic cathode presented a capacity of ∼60 mA h g−1 in a full cell with the hard carbon anode.94 In the case of the rGO cathode, the anions are stored on the surface of graphene sheets, which provides higher capacity and better kinetics.
To demonstrate the feasibility of a reduced graphene oxide cathode, rGO_2 was coupled with a hard carbon anode and a full cell galvanostatic cycling was carried out. The performance of hard carbon anode is presented in Fig. S8 (ESI†). The full cell cycling was performed with a current density of 30 mA g−1 in a narrowed potential window (0.5–3.7 V) to avoid electrolyte decomposition. The upper and lower cut-off voltages were derived from stable half-cell measurements (3.8–1.2 V) and then adjusted to 3.7 V and 0.5 V, respectively, to accommodate the anode's working potential window (0.1–1 V). Only the rGO cathode was presodiated prior to assembly. Fig. 7(A) shows the charge–discharge profiles of cycles 2–11th of the full cell. The charge–discharge curves reflected the sloping shape observed in the half cell. The discharge capacity achieved after the formation cycle was 101 mA h g−1 (based on the cathode active mass). In the first 10 cycles, the capacity was increased to reach 125 mA h g−1. A similar increase was observed for the rGO_2 half cells and can be ascribed to the opening of the rGO structure and the gradual electrolyte penetration into the electrode.22 An additional effect has the balancing of anode and cathode potentials, as the capacity ratio was not perfectly matched. Based on the total mass of the cathode and anode active materials and average discharge potential of 1.85 V, the specific energy of the full cell is calculated to be 80 W h kg−1. For comparison, similar energy density was achieved with the rGO/Sb2S4–Na2/3Ni1/3Mn2/3O2 system, which consists of much more expensive and less sustainable transition metals.95 Moreover, the rGO_2 – HC full cell showed remarkable stability over 500 cycles, which is reflected in a capacity loss of only 0.05% per cycle. Further optimisation of electrode materials, potential windows and electrolytes can significantly improve the energy density.
Detailed in situ Raman spectroscopy and PDF measurements shed light on the electrochemical processes. Both techniques ruled out ion intercalation commonly observed in graphite electrodes. Instead, the energy storage mechanism relied on surface reactions and was divided into two stages, one depending on the Na+ ions intake below 3.5 V, and a second process above 3.5 V, which involved the association of anions from the electrolyte on the rGO surface. It was found that Na+ ions are stored mainly on the defects and edges of rGO as well as via redox reaction with the functional groups: CO + Na+ + e− ↔ C–ONa. Moreover, functional groups containing nitrogen increased the capacity by offering more reaction sites for Na+ ions. At the higher potentials, the perchlorate anions from the NaClO4 salt associate on the graphene basal plane. The N-heteroatoms enhanced the adsorption of ClO4− anions, however also amplified decomposition to NaCl causing severe electrolyte degradation. All these mechanisms are predominantly surface reactions, which ensure good rate capability and high structural stability of electrodes. This also indicates that optimisation of both materials morphology and chemical structure can result in excellent performance.
To avoid severe electrolyte decomposition above 4.2 V, a narrower cut-off potential was applied. Although this resulted in decreased capacity, as the p-doping region was not fully utilized, the cycle life was greatly improved. Therefore, careful selection of more stable electrolytes can make high capacity and long cycle life rGO cathodes possible.
As a proof-of-concept, a full cell with rGO_2/CMC cathode and hard carbon anode was assembled. It showed a specific energy of 80 W h kg−1 and outstanding stability over 500 cycles, proving that rGO is a viable SIBs’ cathode material candidate. Replacing transition metal oxides with carbonaceous cathodes could solve environmental and economic concerns and lead to a significant reduction in the overall manufacturing costs of SIBs. The gained comprehensive understanding of the energy storage mechanism in rGO electrodes can be applied to design high-performance carbonaceous cathodes for SIBs. This can render the commercialisation of all-carbon SIBs viable as a low-cost and sustainable solution for different applications, particularly for medium- to large-scale energy storage.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ma00605d |
This journal is © The Royal Society of Chemistry 2024 |