Magdalena Teresa Spicher*ab,
Sebastian Patrick Schwamingerbcd,
Daniela von der Haar-Leistla,
Marian Montiel Peraltaa,
Georgina Mikacevica,
Friedrich Ernst Wagner‡
e and
Sonja Berensmeierb
aFraunhofer Institute for Process Engineering and Packaging (IVV), Giggenhauser Str. 35, 85354 Freising, Germany. E-mail: magdalena.spicher@ivv.fraunhofer.de; Tel: +49 8161 491459
bChair of Bioseparation Engineering, School of Engineering and Design, Technical University of Munich, Boltzmannstraße 15, 85748, Garching, Germany
cDivision of Medicinal Chemistry, Otto Loewi Research Center, Medical University of Graz, Neue Stiftingtalstraße 6, 8010, Graz, Austria
dBioTechMed-Graz, Austria
eDepartment of Physics, Technical University of Munich, James-Franck-Straße 1, 85748 Garching, Germany
First published on 20th May 2024
Due to its simplicity, co-precipitation is the most commonly used method for producing iron (oxyhydr)oxide nanoparticles. However, it is reported to be sensitive to changes in process parameters, which complicates scale-up and is why only volumes up to 1.2 L have been described in the literature. This study aims to demonstrate the scale-up of a co-precipitation synthesis to 100 L using the example of a new phosphate-binding active ingredient based on iron (oxyhydr)oxide. The synthesis was shown to be very robust to changes in synthesis parameters and stirrer geometries. The in vitro phosphate-binding efficacy and the yield were maintained in all five scales tested. Only the content of the components in the nanoparticles varied slightly. However, Mössbauer spectroscopy, dynamic light scattering (DLS), and attenuated total reflection Fourier transform infrared spectroscopy (FT-IR) revealed no evidence of structural changes, but a reduction in the size of the iron (oxyhydr)oxide cores and the total core–shell nanoparticle sizes. Overall, this study has successfully demonstrated that ultrasmall iron (oxyhydr)oxide nanoparticles can be produced on a pilot scale by co-precipitation with a yield of >40 g L−1.
Various synthetic methods are known for preparing iron (oxyhydr)oxide nanoparticles, such as microemulsion systems, sol–gel technique, and hydrothermal synthesis.12 Due to its simplicity, co-precipitation synthesis is the most commonly used method based on the precipitation of ferric and ferrous ions dissolved in water by adding a base.5,6,12 However, it is well-known that numerous influencing factors in co-precipitation synthesis affect the product properties, like the stirring speed, temperature, or the addition time of both reactant solutions.6,13–15 On the one hand, this enables the preparation of a wide range of tailored iron (oxyhydr)oxide nanomaterials with various crystal structures and different particle sizes and shapes.14 On the other hand, it requires precise synthesis control due to the lower robustness of the process, complicating the scale-up of co-precipitation syntheses and can lead to potential impairment of factors like particle size, product purity, colloidal stability, or surface morphology.16 Thus, the synthesis procedures following the co-precipitation route are typically described in research studies with small volumes of up to 1 L and a small amount of product.11,17–20 The largest reported co-precipitation process syntheses are in the range up to 1.2 L total volume and 5.4 g L−1 of product.21,22
To our knowledge, no study has reported a transfer from the laboratory to larger scales and the challenges associated with the scale-up yet. This study aims to demonstrate that ultrasmall iron (oxyhydr)oxide nanoparticles can be produced at a pilot scale-up to 100 L reaction volume despite the sensitivity of co-precipitation synthesis. We perform the scale-up using the example of the production of a newly developed, potentially highly effective active ingredient for the treatment of hyperphosphatemia.23 This drug consists of ultrasmall (<20 nm) iron (oxyhydr)oxide nanoparticles enclosed in an organic shell composed of inulin, mannitol, and gum arabic.24 The synthesis of this nanoparticle material has been described up to now only for a total volume of 0.2 L with about 8–10 g of product amount.24 In this study, we investigate the robustness of the process on a laboratory scale and then transfer the synthesis stepwise up to a reaction volume of 100 L with a production of at least 40 g L−1 without limiting the outstanding efficacy of the novel active ingredient.
Fig. 1 Schematic illustration of the manufacturing process subdivided into (a) particle preparation by co-precipitation and oxidation, and (b) further processing of the nanoparticle suspension. |
The production is divided into two sections: (a) particle preparation by co-precipitation synthesis and (b) further processing to refine the particles. This work focuses on section (a). The further steps of section (b) are consistently performed according to the procedure of the laboratory process.24 Upscaling of the further steps is part of further studies.25,26
The nanoparticle synthesis was performed in 5 scales from a total reaction volume of 180 mL to 100 L (see Table S1 in the ESI†). The quantity of all solutions used for the preparation can be found for the different scales in Table S1.† The reaction tanks were glass tanks on smaller scales and stainless steel tanks on larger ones (see Table S1†). We use counter-current stirrers with a power input of 18 W m−3 (except for 0.2 L, where a propeller stirrer with a power input of 160 W m−3 was used). Temperature control was performed using the double-walled reaction vessels with externally connected thermostats. The scale-up was carried out, as far as possible, according to the similarity principle.27 From a reaction volume of 1.8 L, the geometric similarity was respected. The agitator geometry and dimensional ratios (ratio agitator diameter/vessel diameter and ground clearance to vessel diameter) were kept constant. In addition, the power consumption per unit volume was kept constant in all scales, as recommended for dispersion processes.27 At least two independent syntheses were performed at each scale.
Synthesis parameter | Description | Level −1 | Level 0 (standard conditions) | Level 1 | Level 2 |
---|---|---|---|---|---|
Temperature (°C) | Temperature during the co-precipitation (step 1) and the first half of the oxidation (step 2) | — | 4 | 25 | 40 |
Power input (kW m−3) | Adjusted by the stirring rate during the complete synthesis (steps 1 and 2) | 0.03 | 0.16 | 0.93 | — |
Titration time (min) | Addition rate of solution 1 to solution 2 at the beginning of step 1 | — | 0 | 6 | 12 |
Co-precipitation time (min) | Duration of step 1 (after the addition of solution 1 to solution 2 until the addition of hydrogen peroxide) | 10 | 15 | 20 | 30 |
Oxidation time (min) | Duration of step 2 (after reaching 60 °C for the oxidation) | 10 | 15 | 20 | — |
After synthesis, the samples were further processed according to the procedure described above under section “Further processing of the active ingredient nanoparticles”. At least three independent syntheses of each parameter combination were performed.
Characteristic | Propellera | Impeller | Diska | Pitched-blade | Counter-current |
---|---|---|---|---|---|
a Tested as single- and two-stage stirrer. | |||||
Number of blades | 3 | 3 | 6 | 4 | 2 |
Stages | 1 and 2 | 1 | 1 and 2 | 1 | 2 |
Primary conveying direction | Axial | Radial | Radial | Axial, radial | Axial, radial |
Recommended viscosity range (Pa s) | <0.5 | <0.5 | <0.5 | <0.5 | 0.5 to 5 |
Agitator diameter d (cm) | 4.0 | 7.4 | 4.4 | 4.3 | 7.4 |
Distance to the bottom of the vessel (cm) | 4.0 | 0.9 | 4.4 | 3.0 | 1.1 |
Stirring speed n (min−1) | 467 | 150 | 186 | 261 | 158 |
The stirrer speed was individually adapted for all stirrers to achieve a power input P/V of 18 W m−3 according to eqn (1).
(1) |
(2) |
The content of total iron β(Fe) and ferrous content β(Fe2+) were determined by a 1,10-phenanthroline colorimetric assay. For the quantification of β(Fe), 22.5 to 50 mg active ingredient was dissolved with 1 mL hydrochloric acid and diluted to 0.5 L with water. 0.98 mL of a phenanthroline reagent solution (1 g per L 1,10-phenanthroline hydrochloride monohydrate, 14 mL per L acetic acid, and 21.7 g per L sodium acetate trihydrate in water) was mixed with 0.28 mL sample solution and 0.14 mL hydroxylamine hydrochloride solution. For the quantification of β(Fe2+), 250 to 500 mg active ingredient was dissolved with 1 mL dilute sulfuric acid (50% in water) and 1 mL ammonium fluoride solution (5 mol L−1 in water) before diluting the sample solution with water to 50 mL. For the analysis, 0.9 mL of the phenanthroline reagent solution (composition see above) and 0.1 mL of the ammonium fluoride solution was mixed with 0.1 mL sample solution. We measured the absorbance of the sample solutions at 510 nm with a BioTek Synergy HTX Microplate Reader and calculated β(Fe) and β(Fe2+) using calibration curves obtained with iron reference solutions. We used solutions of iron standard diluted in water (for the quantification of β(Fe)) and diluted in 240 mL per L hydroxylamine hydrochloride solution (for the quantification of β(Fe2+)). The share of ferrous ions c(Fe2+) was calculated as follows:
(3) |
We used high-performance anion exchange chromatography, as previously described by Spicher et al.,4 to quantify mannitol and inulin. The Dionex ICS-3000 Ion Chromatography System was equipped with a pulsed amperometric detector, a CarboPac PA10 column (Thermo Fisher Scientific) and a guard column (Thermo Fisher Scientific). Eluent A was water, eluent B 150 mM NaOH and eluent C 150 mM NaOH with 1 M sodium acetate. The flow rate was 0.25 mL min−1 with a temperature of 25 °C. For the measurements, the eluents were mixed as follows: 0–25 min: 90% A + 10% B; 30–35 min: 100% C; 40–55 min: 90% A + 10% B. 50 mg active ingredient was mixed with 1.5 mL 2% hydrochloric acid and heated to 80 °C for 60 minutes. 30 μL of this solution was diluted with 0.1 M sodium hydroxide to 10 mL and 500 μL was mixed with 1.5 mL internal standard solution (10 g per L sodium azide and 0.2 g per L maltitol in water). Before analysis, all sample solutions were filtered with a 0.2 μm nylon syringe filter. The content of mannitol β(Man) and inulin β(Inu) was determined using calibration curves measured with standard solutions containing glucose, fructose, and mannitol. β(Inu) was calculated as the sum of the contained glucose and fructose amount.
The chloride content β(Cl) was determined using a mercuric thiocyanate photometric assay using a chloride test kit (Hach Company), according to Spicher et al.25 We dissolved 30 mg of the active ingredient with 2 mL 3% nitric acid within 10 min at 80 °C. For the quantification, we used a standard addition method: we added defined amounts of 0 to 3 μL chloride standard solution (1000 mg L−1) to the sample solutions and diluted the mixtures to 1 mL with water. For the spectroscopic measurement, 160 μL mercury thiocyanate solution and 80 μL ferric ion solution, both contained in the test kit, were added to the samples, and the absorbance at 455 nm was measured with a BioTek Synergy HTX Microplate Reader. β(Cl) was calculated by linear regression.
The residual moisture RM was determined by Karl Fischer titration using a Karl Fischer KF titrator Aqua 40.00 (ECH Elektrochemie Halle GmbH) equipped with a headspace module. 10 to 20 mg of the active ingredient was filled in a headspace vial, sealed with an aluminum cap, and heated in the headspace module to 90 °C. The evaporation moisture was quantified until the following drift stabilization was achieved: increase ≤ initial drift + 2 μg min−1.
(4) |
In addition, we calculated the volumetric binding capability M(PO43−), which correspond to total mass of phosphate that could be bound with the active ingredient produced per L synthesis volume, according to eqn (5). M(PO43−) enables to compare the effect of a different synthesis yield and binding efficacy (e.g. for an active ingredient sample with a low synthesis yield but with a high phosphate-binding efficacy).
(5) |
The results can be found in Tables S2–S6 in the ESI.† The most critical characteristics of the process are the product yield and the in vitro efficacy (as well as the volumetric binding capability). No significant differences are observed for these characteristics when the synthesis parameters are varied. The mean values of all samples are shown in Table 3.
Characteristics | Average |
---|---|
Synthesis yield Y (g L−1) | 47.4 ± 3.0 |
Phosphate-binding efficacy q(PO43−)pH 3 (mg g−1) | 200.0 ± 12.2 |
Phosphate-binding efficacy q(PO43−)pH 7 (mg g−1) | 122.2 ± 12.1 |
Volumetric binding capability M(PO43−)pH 3 (g L−1) | 9.4 ± 0.8 |
Volumetric binding capability M(PO43−)pH 7 (g L−1) | 5.8 ± 0.7 |
Regarding the composition, some minor changes in the iron and inulin content can be recognized. The inulin content rises with increasing synthesis temperature, power input, and titration time (see Tables S2–S4 in the ESI†). The iron content, on the other hand, decreases with increasing power input and longer co-precipitation time (see Tables S3–S5 in the ESI†). However, comparable research studies typically only consider the effects on the particle size distribution and the formed crystal structures6,14,15,35 but not on the composition of the nanoparticles. We suspect that the observed effects could also be due to variations in the primary particle size or shape. The iron ions are expected to be bound in an iron (oxyhydr)oxide structure in the core of the nanoparticles.24 The organic components surround this core as a shell, protecting the nuclei from particle aggregation. A change in the ferrihydrite core size leads to a different volume/surface area ratio, whereby the quantity ratio of iron and organic components can vary. Due to the above-mentioned limited sample quantity, which already forced us to forego a complete analysis of the composition, we could not additionally perform a size determination of the ferrihydrite cores.
Furthermore, it still needs to be clarified in which range the composition of the active ingredient may vary to achieve a constant yield and phosphate-binding efficacy. Since a comparable yield and phosphate-binding efficacy were observed in this test series, we estimate a relatively small effect of the composition. To verify this, we determined possible correlations between the content of the components and the efficacy and yield using statistical correlation analyses. The results are shown in detail in Table S7 and Fig. S1 in the ESI.† Significant correlations were identified between the content of inulin and mannitol (see Fig. 2a) and between the iron content and the product yield (see Fig. 2b), as well as the phosphate-binding efficacy (see Fig. 2c and d).
The results indicate that active ingredient samples with a higher mannitol content have a significantly lower inulin content. Both organic substances are expected to bind to the surface of the iron (oxyhydr)oxide core via ligand exchange reactions and electrostatic attraction forces.24 They thus compete for the same binding sites, which is why a negative correlation in the content of these two molecules can be observed.
Furthermore, the data demonstrate that a higher iron content leads to a lower yield and, at the same time, to a higher phosphate-binding efficacy (see Fig. 2b–d). Regarding the reduced yield, we assume that particles with a higher iron content are less stabilized and thus tend towards particle growth and aggregation.36 As a result, a bigger fraction of particle aggregates is separated in centrifugation in this manufacturing process, which is why the product yield is reduced. The positive influence of the iron content on the phosphate-binding efficacy can be explained by the binding mechanisms of phosphate to iron (oxyhydr)oxides. In general, two possible mechanisms are distinguished: phosphate ions can bind to surface iron ions via adsorption and can cause iron ions to dissolve out of the iron (oxyhydr)oxide structure and precipitate to iron phosphate.37–41 For the active ingredient of this study, Spicher et al. recently reported evidence of both binding mechanisms in phosphate-binding.4 In samples containing more iron, more binding sites are available to the phosphate, so that a higher phosphate-binding efficacy can be observed. However, the results of this study also showed that the iron content alone is not decisive for the exceptionally high efficacy, but that the organic components in the active substance also seem to play a decisive role.4 But the authors could not finally clarify this connection in their study. The reported results support our observations that, despite minor changes in composition, all samples produced showed comparable efficacy.
Considering these results in the synthesis scale-up, it is particularly worth mentioning that the iron content has an opposite effect on the target parameters yield and phosphate-binding efficacy. While an increasing iron content leads to an increase in efficacy the amount of product decreases simultaneously. It is not possible to make a general conclusion whether a higher yield with a lower efficacy or a lower yield is economically preferable. For this reason, we additionally calculated the volumetric phosphate-binding capability M(PO43−), which indicates the total amount of phosphate the active ingredient per L synthesis can bind. It combines the synthesis yield and the phosphate-binding efficacy in one factor. The correlation analysis indicates no dependence of M(PO43−) with iron content (see Table S7 in the ESI†).
In summary, we found no significant changes in yield and phosphate-binding efficacy by changing the synthesis parameters. Only slight differences in the inulin and mannitol content were observed. Subsequent correlation analyses indicated that only the iron content affected the yield and the phosphate-binding efficacy. However, particle composition does not significantly influence the volumetric phosphate-binding capability. For this reason, the synthesis is overall very robust and not very sensitive to changes.
Based on the general characteristics of the most common agitator geometries for liquid media, we have made a preselection whereby the recommended viscosity range was decisive. Between 4 °C and 60 °C, the synthesis suspension containing the iron (oxyhydr)oxide nanoparticles has a dynamic viscosity lower than 10 mPa s (see Fig. S2 in the ESI†). For this reason, we excluded stirrer geometries that are more suitable for more viscous media, such as the anchor stirrer.28 We selected five different stirrer designs (propeller, impeller, disk, pitched blade, and counter-current type) to empirically test their suitability for mixing during the co-precipitation synthesis. In addition, we tested the propeller and the disk agitator as one- and two-stage stirrers.
The active ingredients produced with the different stirrers are all similar in their properties (see Table S8 in ESI†). No significant differences are observable in the composition, the phosphate-binding efficacy, and the synthesis yield, and the parameters are consistent with the observed results of the robustness study (see Table 4).
Characteristics | Average |
---|---|
Synthesis yield Y (g L−1) | 43.0 ± 4.3 |
Phosphate-binding efficacy q(PO43−)pH 3 (mg g−1) | 204.7 ± 10.6 |
Phosphate-binding efficacy q(PO43−)pH 7 (mg g−1) | 110.0 ± 9.6 |
Volumetric binding capability M(PO43−)pH 3 (g L−1) | 8.8 ± 1.1 |
Volumetric binding capability M(PO43−)pH 7 (g L−1) | 4.8 ± 0.8 |
In summary, all tested agitator types are equally suitable for producing the active ingredient on larger scales. For the further scale-up, we selected the counter-current stirrer.
The mean synthesis yield, the phosphate-binding efficacy, and the volumetric binding capability are in good agreement with the observed results of the preliminary studies reported above (see Table 5).
Characteristics | Average |
---|---|
Synthesis yield Y (g L−1) | 43.7 ± 6.5 |
Phosphate-binding efficacy q(PO43−)pH 3 (mg g−1) | 196.8 ± 17.2 |
Phosphate-binding efficacy q(PO43−)pH 7 (mg g−1) | 122.3 ± 17.5 |
Volumetric binding capability M(PO43−)pH 3 (g L−1) | 8.5 ± 1.4 |
Volumetric binding capability M(PO43−)pH 7 (g L−1) | 5.3 ± 1.1 |
We also examined the composition of the active ingredient samples, like in the preliminary tests (see Table S9 in the ESI†). Significant differences in the inulin, mannitol, and iron content were found, changing with the synthesis scale, graphically illustrated in Fig. S3 in the ESI.† A systematic increase can be noticed with increasing synthesis scale for the inulin and the mannitol content. Whereas on the laboratory scale, only 120 ± 10 mg per g mannitol and 136 ± 8 mg per g inulin were contained in the active ingredient samples, the content of both substances increased up to 162 ± 4 mg per g mannitol and 228 ± 24 mg per g inulin after synthesis with 100 L total volume. At the same time, a slight reduction in the iron content from 216 ± 4 mg g−1 in the laboratory scale to 194 ± 6 mg g−1 in the 100 L-synthesis can be observed.
To exclude changes in structure, we recorded FT-IR spectra of the active ingredient samples of all synthesis scales (see Fig. 4).
Fig. 4 Fourier transform infrared (FT-IR) spectra of active ingredient samples synthesized in different scales. |
There are only slight differences observable in the spectra. The samples produced on the larger scales show a higher peak at 938 cm−1, and the shoulder between 1150 and 1090 cm−1 is more prominent. These changes can be attributed to the increased inulin content in the active ingredient samples produced on larger scales.25 Furthermore, the peaks at 1065 and 1035 cm−1 change with the synthesis scale. In this wavelength range, mannitol, inulin, and gum arabic show peaks caused by C–O–C stretching.42–44 As recently reported, different content ratios of these three organic components lead to altered shapes of these two peaks.25 Lastly, the peak at 1600 cm−1 decreases with increasing synthesis scale. This peak is a typical vibration of molecular water in ferrihydrite,45 the most probable crystal structure of this active ingredient.24 Thus, the spectra indicate a decrease in the ferrihydrite content with the synthesis scale, which is consistent with the observation of the reduction of the iron content and the increase of the organic components. It is also conceivable that the ferrihydrite content is reduced by forming other iron (oxyhydr)oxide structures. Usually, X-ray diffraction (XRD) is applied to study the crystal structure in this type of nanomaterial.46
However, it has already been shown in a preliminary study that XRD analyses are challenging for this active ingredient due to the ultrasmall particle size and the low crystallinity.24 Instead, Bäumler et al. applied Mössbauer spectroscopy, among other methods, to further characterize the iron (oxyhydr)oxide core of this compound.24 To obtain information on the environment of the iron ions and thus derive conclusions on potential changes in the crystal structure, we also investigated the active ingredient samples produced on the 100 L scale with this method (see Fig. 5). For comparison, we use the results presented by Bäumler et al. on the characterization of this active substance.24 The samples analyzed in that study were prepared on a laboratory scale with a synthesis volume of 176 mL according to the procedure described above in section “preparation of the nanomaterial”.
Fig. 5 Mössbauer spectra of the two active ingredient samples prepared on a pilot-scale (100 L), and the reference sample, produced on a laboratory scale (176 mL, data reproduced by Bäumler et al.24) measured at (a) 300 K, and (b) 4.2 K. |
At 300 K, the Mössbauer spectra of both samples show a doublet with an isomer shift of 0.25 mm s−1 and an average electrical quadrupole splitting of 0.85 mm s−1. The doublet spectra is characteristic of the high spin of Fe3+.24 There is no evidence for the presence of Fe2+. This is in good agreement with the photometrically determined Fe2+ content of less than 1.5% of the total iron (see Tables S2–S9†). They are almost identical to the Mössbauer spectrum of the laboratory-scale drug sample.24 Likewise, the spectra recorded at 4.2 K compare well with the laboratory scale sample. Both samples from the 100 L syntheses show a magnetic sextet with an isomer shift of 0.24 mm s−1 and a mean electrical quadrupole splitting of −0.03 mm s−1, comparable to the laboratory scale reference sample.24 Only the mean hyperfine field of the pilot-scale samples of 44.0 and 44.4 T is slightly lower than that of the reference sample of 45.8 T. It is generally known that the hyperfine field at 4.2 K of iron (oxyhydr)oxides is reduced with decreasing particle size as the anisotropic energy of the particles is raised.47 Therefore, it is reasonable that the particles from the pilot-scale have slightly smaller crystal nuclei than those from the laboratory scale. These findings are in good agreement with the total particle size. Dynamic light scattering analyses reveal a significant reduction in particle size with increasing synthesis volume (see Tables S9 and Fig. S4†). In TEM images, it can be recognized that despite ultrasonic suspension, the ultra-small nanoparticles are not isolated, but are present in particle agglomerates consisting of individual small, dark, crystalline dots (iron (oxyhydr)oxide cores) in a lighter matrix (organic shells) (see Fig. 6a and b). However, the TEM images do not allow an accurate size estimation of the particle cores due to the agglomerates. Overall, the results of Mössbauer spectroscopy and DLS are consistent with the observation that particles from larger synthesis scales have a higher proportion of organic components. As discussed above, larger surface/volume ratios are expected with smaller crystal cores, wherefore more organic molecules can be bound to the ferrihydrite core. As a result, the total particle size is decreasing.
Fig. 6 Transmission electron microscope (TEM) images of the iron (oxyhydr)oxide-based nanoparticles. |
In summary, the FT-IR spectra show only minor changes in peak heights without new peaks, and the Mössbauer spectra are almost identical to those of the laboratory scale. Thus, ferrihydrite still seems to be the iron (oxyhydr)oxide structure in the core without any structure change due to the scale-up. However, there is evidence that the ferrihydrite core has decreased in size, presumably allowing more organic molecules to bind to the core surface. Therefore, the inulin and mannitol content in the particles has probably increased while the iron content has decreased. No significant changes are evident due to the scale-up for the essential properties, the yield, and the phosphate-binding efficacy. Overall, the results thus prove that these ultrasmall iron (oxyhydr)oxide nanoparticles can be successfully produced on a pilot scale.
Based on these results, the scale-up is considered to be successful. However, follow-up studies should be conducted to investigate in detail if the in vivo efficacy is not affected by the composition variation, especially regarding an increased inulin and mannitol content.
Overall, this successful scale-up demonstrated that ultrasmall iron (oxyhydr)oxide nanoparticles with almost constant properties and in vitro efficacy, as well as a yield > 40 g L−1, can be produced on a pilot scale by co-precipitation. These results support overcoming the obstacle of producing large quantities of nanoparticles by co-precipitation to exploit tailored iron (oxyhydr)oxide nanomaterials.
Footnotes |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d4ra02719a |
‡ Deceased during preparation of the manuscript. |