Filomena
Salvemini†
*a,
Francesco
Grazzi
a,
Nikolay
Kardjilov
b,
Ingo
Manke
b,
Francesco
Civita
c and
Marco
Zoppi
a
aConsiglio Nazionale delle Ricerche, Istituto dei Sistemi Complessi, Sesto Fiorentino (FI), Italy. E-mail: filomena.salvemini@ansto.gov.au
bHelmholtz Zentrum Berlin, Hahn-Meitner Pl. 1, 14109 Berlin, Germany
cMuseo Stibbert, Firenze (FI), Italy
First published on 5th November 2014
Computed laminography (CL) has been developed as a method to complement computed tomography for three-dimensional imaging of laterally extended specimens. Originally applied for medical purposes, more recently CL has been used as a non-destructive method, not only in the materials science research, but also with rising interest in artwork investigations. Here, we report the implementation of computed laminography with polychromatic and monochromatic neutron radiation carried out on five historical and archaeological metal artefacts pertaining to different periods and technological contexts. The measurements were performed at the CONRAD II neutron imaging facility at the BERII research reactor of Helmholtz-Zentrum Berlin (HZB).
In order to overcome this drawback, Computed Laminography (CL) was developed as a method to complement computed tomography for three-dimensional imaging of laterally extended specimens. In the typical laminography set-up, the sample rotation axis is tilted with respect to the standard tomographic rotation axis that is oriented perpendicular to the beam. The extended sample plane is then arranged approximately perpendicular to the rotation axis as shown in Fig. 1. The advantage of this scanning scheme is that the integral transmission stays almost constant for the full set of angular projections. As a consequence, the integrity of laterally extended samples can be preserved.9,10
Early use of laminography with X-rays was in the field of medical applications.11 Recently neutron computed laminography has been applied also to materials science research12 and the interest in the application of the technique to art or archaeological objects rose since such samples require investigation through non-invasive methods.13,14
However, this technique can be further improved, to achieve material discrimination, by a proper selection of the neutron energy. In fact, monochromatic neutron beams give the possibility of modifying the image contrast for different phases taking advantage of the abrupt change of the attenuation coefficients in the proximity of the so-called Bragg edges.15–17
Considering the potential of laminography for implementing the status of knowledge about ancient technology, the purpose of this study was to examine expanded applications of these non-invasive methods. These studies include the use of different neutron laminographic methods which would allow for reconstruction and imaging of ancient metal artefacts. Neutron white beam laminography (WBL), and for the first time, energy-selective laminography (ESL) were performed on the CONRAD II beam line at HZB.
Fig. 2 (a) The iron tsuba, (b) the copper tsuba, (c) the Celtic spiral, (d) the fuchi 01 and (e) the fuchi 02 are reported. |
The first tsuba (Fig. 2a) is a slightly elliptical iron one with a rounded rim. The tsuba is carved with a tendril design (sukashi technique), including facing dragons, a jewel, and stylized flowers. The rim is rounded and gilded and there are traces of gilding in other areas. It is not signed but can be dated to the first half of the XVIIIth century, probably from the Nagasaki (Hizen) area, in namban style. The Japanese word namban, translated as “southern barbarian”, was used by Japanese not only to indicate any foreigner who entered their country, but also to define a large number of artworks in which the decorations reflected a foreign influence in their appearance. The diameter of 8 cm leads us to presume that this hand-guard was created for a long sword (katana). It was equipped with a nakago hitsu, the central hole for fitting the tang of the blade, and a kozuka hitsu, the left side hole for accommodating the handle of a small knife called kozuka.
The second Japanese hand-guard was made of copper and copper alloys (Fig. 2b) and is of sanmai type: this is composed of three layers with the central one made of a different alloy with respect to the others. The upper and lower layers are decorated through hammering. Decoration was typically made by acting on the back of the layer and then fastening it to the central layer with adhesive or lacquer. A fukurin, i.e. soft metal, type rim was hammered around to hold the three layers together. The rim profile is rounded and not decorated. The decoration theme is made of waves and imaginary animals (dragons). The piece can be dated either to the end of the Momoyama period or to the beginning of the Edo period. It was probably made in the Kyoto area around the beginning of the XVIIth century. A relief decoration is visible on the surface even though it is in poor conditions of conservation. Detachments are recognizable at the edge and on the decorated surface. As in the previous sample, there is a nakago hitsu and a kozuka hitsu.
The other samples are a bronze Celtic spiral, showing the typical alteration products of copper on its whole surface (Fig. 2c), together with two fuchi (Fig. 2d and e) made of copper and copper alloys.
Bronze was extensively employed by the Celts to make a wide variety of objects and this metal alloy was especially common for jewellery. Brooches, buckles, belt ends, dress pins and rings could be obtained by simply cold-working the metal blank or applying complex inlay techniques.20 In the case of our sample, the spiral, one of the most used patterns by Celts, was probably made out of a bronze wire that was bent to form a spiral into a looped circular shape. The sample was found in England and dated to the 1st millennium BC.
Regarding the fuchi, it has the mechanical function to strengthen the hilt of the blade at the conjunction with the tsuba. The ordinary fuchi consists of a flat band of metal up to half an inch wide that encircles the hilt immediately below the guard. As any component in a Japanese sword mount, it is easily removable. Its base is filled with an oval plaque, usually copper, pierced with a hole to insert the tang. The two fuchi analysed in this work are both manufactured during the Edo period.
In order to place the samples in the beam, an aluminium threaded rod was gently passed through the main hole (nakago hitsu) of the two tsuba and fastened with an iron bolt. Small Al plates were placed between the sample surface and the bolt in order to avoid direct contact that could affect the data processing and damage the objects. Concerning the Celtic spiral, due to its bad conservation conditions and to the shape, this sample was wrapped in aluminium foil and fixed on an Al plate mounted on the top of the rod (Fig. 3a). The very low macroscopic cross-section of aluminium makes this metal almost transparent to neutrons and avoids interference during the measurements. The rod, with the samples fixed along it, was connected to the rotating table and placed on a goniometer. The rotation axis of the samples was tilted 20 degrees towards the detector as shown in Fig. 3b and angular projections were measured at stepwise rotation over 360 degrees. The measured projections were reconstructed by the laminographic method using the software package Octopus21 and visualized using VGStudio Max.22
The experimental conditions for the performed different experiments are presented in Table 1. White beam laminography was performed only on the two tsuba and the Celtic spiral, instead, the two fuchi were chosen for the energy-selective laminography on the base of following considerations. As evidenced by previous neutron diffraction analysis, these samples have a composite copper and copper-alloy structure. Moreover, a non-homogeneous distribution of the neutron wavelengths inside the acquisition window could be experienced when the neutron beam is monochromatized. This implies a gradient of wavelength which distribution and extension depend on the type and arrangement of the selector device (details will be discussed elsewhere). Considering the high wavelength resolution required to detect the different metal alloys of interest (they have a similar composition and a very close phase lattice parameter), only the two fuchi, whose size is below the range of the wavelength shift in the acquisition field, were analyzed.
W-B laminography | Radiography E scan | E-S laminography | |
---|---|---|---|
Wavelength | Polychromatic | From 2.0 Å to 4.5 Å with a step of 0.02 Å | 4.18 Å/4.21 Å/4.30 Å |
Camera | Andor DW436N-BV CCD3325 2048 × 2048 16 bit | ||
Scintillator | LiF 50 μm | LiF 400 μm | LiF 400 μm |
L/D | 500 | 333 | 333 |
FOV | 110 × 110 mm | 200 × 200 mm | 111.5 × 111.5 mm |
Sample–detector distance | 90 mm max. | 20 mm | 90 mm max. |
Pixel size | 53.8 μm | 106 μm | 54.45 μm |
Exposure time | 60 s | 150 s | 130 s |
Projection # | 600 | — | 300 |
Tomo angle | 0–360° | — | 0–360° |
Tilt angle | 20° | — | 20° |
Flat field # | 20 | 1 × wavelength | 10 × wavelength |
Dark field # | 20 | 10 | 10 |
The white beam laminography revealed a homogeneous body for the iron tsuba, probably filed starting from a single piece of iron (Fig. 4). As a matter of fact, starting from the Muromachi period, the sukashi technique evolved over time. The iron plate prepared as the ground metal was very uniformly forged and relatively soft in order to cut out the fine designs successfully but hard enough to avoid breakage during use. Any void or significant irregularity in the iron body would have made the shaping of continuous decorative lines impossible. Extra effort in the preparation of the plate would have been necessary, as observed in the inner volume of the samples which was free from any cracks, pores and inclusions.23 Evidence of forge-welding was not identified in the design motifs involving plant and animal figures, apart from the gilded ring outlining the profile of the kozuka hitsu. While the inner brighter areas are reconstruction artefacts, the ones detected on the surface were probably due to the application of a patina or to the early formation of products of alteration.24
Virtual cross-sections taken at different heights of the copper tsuba revealed three layers of copper and copper alloys (Fig. 5). According to the ancient metal working technique described in the literature,25 the external sheets of metal were probably applied on the two sides of the inner core by heating and slightly hammering, while their rather soft surface was worked with a punch to give texture. All around the rim of the tsuba and the pierced hole, the composite structure was finally tightened by applying a thin ring appearing detached and lost in some areas.
The laminography allowed reconstruction of the whole inner volume of the Celtic copper spiral, entirely covered by alteration products (Fig. 6). A qualitative elemental characterization of the sample has been performed. Taking into account the neutron wavelength distribution of the probing beam and the image slope value, the total neutron macroscopic cross-sections (absorption and scattering) of Cu and H have been estimated. On the basis of the calculated threshold value between copper and hydrogen, the segmentation of the image histogram allowed us to distinguish the still intact metal, inside the sample, and the alteration, covering the surface and diffusing into the metal. The intact metal is visible inside as well as the dark areas that, according to shape and extension, are probably related to the presence of porosity. The detected structure of the artefact is simple and was obtained by wrapping a wire of copper around itself.
Preliminarily to the ESL, radiographic energy scan was carried out aiming to discriminate the presence of copper and copper alloy materials by exploiting the contrast enhancement obtained using different neutron wavelengths (Table 1, central column). In particular, to fulfil this task, we used neutron wavelengths at values immediately above and below the 111 Bragg-edge for Cu and Cu-alloys,29 according to the lattice parameter defined by previous neutron diffraction analysis (Table 2). We recall that the copper alloys maintain the same lattice structure of pure copper (FCC) while the lattice parameter changes according to the amount and type of solute mixed in it.30
(a) | |
---|---|
hkl | 2d = λ (Å) |
111 | 4.18 |
200 | 3.62 |
220 | 2.56 |
311 | 2.18 |
222 | 2.09 |
400 | 1.81 |
(b) | ||||
---|---|---|---|---|
Cu | Cu-alloy | |||
a o | Δao | a o | Δao | |
Tsuba | 3.6158 | 0.0004 | 3.693 | 0.001 |
Fuchi 01 | 3.61829 | 0.00002 | 3.6279 | 0.0004 |
Fuchi 02 | 3.61857 | 0.00002 | 3.6251 | 0.0006 |
(c) | |||
---|---|---|---|
a o | d (111) | Bragg-edge (Å) | |
Cu | 3.617 | 2.088 | 4.176 |
Cu-alloy | 3.649 | 2.107 | 4.214 |
Energy scans have been performed from 2.0 Å to 4.5 Å with steps of 0.02 Å, crossing the 111 FCC Bragg edge for copper and for copper alloys. Fig. 7 reports the optimum neutron wavelength values above and below the Bragg edges at which the highest intensity variation have been found (i.e. 4.18 Å and 4.22 Å).
In order to increase the statistics, each laminographic stack was processed by applying a median filter over 50 slices along the z axis.
According to the neutron diffraction results reported in Table 2c, and the energy scan shown in Fig. 7, the Bragg edges for copper and copper-alloy are approximately located at 4.18 Å and 4.22 Å. Applying the method described in ref. 5, which is omitted from here for the sake of conciseness, the change in the transmission spectrum at the Bragg-edge correspondence has been exploited to recognize the distribution of copper and copper-alloy. The presence of Cu has been evidenced by subtracting the 4.15 (above the Cu 110 Bragg edge) from the 4.21 Å image (below the Cu 110 Bragg edge). Similarly, Cu-alloy-based elements were mapped by subtracting the 4.21 Å (above the Cu-alloy 110 Bragg edge) from the 4.30 Å (below the Cu-alloy 110 Bragg edge) image.
The same procedure was followed for both fuchi. In the case of sample F01, the image resulting from subtracting the stack above and below the copper Bragg edge (Fig. 8, F01, first sequence – image 4.15–4.21 Å) evidenced, in the brighter grey tone, the presence of a flat pale made of Cu. A collar surrounded by decorative elements of a Cu-alloy-based material can be pointed out in the brighter area of the image 4.21–4.30 Å (Fig. 8, F01, second sequence).
Similar results were evidenced for the sample F02, featuring a copper collar outlined by a Cu-alloy material (Fig. 8, F02).
Neutron white beam and energy-selective laminographies were used for the non-invasive investigation of laterally extended specimens and for showing the validity of the proposed laminographic methods. Moreover, the contrast enhancement induced by the selection of an appropriate neutron wavelength was exploited to increase the image contrast for the different material containing the analyzed specimens.
White beam laminography allowed identification of peculiar characteristics related to the manufacturing methods of these flat objects:
■ the inner structure, resulting from the particular manufacturing process, was analysed all over the samples;
■ the presence of possible forge-welding and soldering was mapped;
■ patination of the surface was established;
■ alterations, originating from the surface and extending to the body of the sample, have been identified for assessing the conditions of conservation.
Concerning the energy-selective laminography, the present measurements demonstrate that the proposed method can allow characterization of the inner structure and composition of metal artefacts, non-destructively, in combination with other neutron inspection techniques.
However, further work is needed to improve the methods. In particular, higher homogeneous distribution in the whole neutron field of view is needed to characterize quantitatively the phase distribution in the case of flat samples made of Cu and Cu alloys.
Footnote |
† Current affiliation: Bragg Institute, Australian Nuclear Science and Technology Organisation (ANSTO), New Illawarra Road, Lucas Heights NSW, Australia. |
This journal is © The Royal Society of Chemistry 2015 |