Jun Qu*a,
Xiaoman Hea,
Xuewei Lia,
Ziqiang Aia,
Yujie Lia,
Qiwu Zhang*a and
Xinzhong Liub
aSchool of Resources and Environmental Engineering, Wuhan University of Technology, Luoshi Road 122, Wuhan, Hubei 430070, China. E-mail: zhangqw@whut.edu.cn; forsjun@whut.edu.cn; Tel: +86 17771490085
bCollege of Ecological Environment and Urban Construction, Fujian University of Technology, Fuzhou 350118, China
First published on 21st June 2017
An amorphous photocatalyst was prepared via simple dry milling of Zn basic carbonate (Zn4CO3(OH)6·H2O) and Al hydroxide (Al(OH)3) as a precursor of Zn–Al layered double hydroxide (LDH) and the precursor was agitated in water to simply synthesize the Zn–Al LDH for comparison. The adsorption and photocatalytic activity of the Zn–Al LDH and the precursor were studied via the removal of methyl orange (MO) and decoloration of MO under ultraviolet light irradiation in aqueous solution, respectively. The precursor exhibits much higher decoloration efficiency towards MO than the Zn–Al LDH product because of the synergistic effect of the intercalation reaction and its photocatalytic activity. The amorphous precursor could easily incorporate MO molecules to form MO intercalated LDH, allowing easy access of the organic pollutant to the photocatalyst sample, resulting in an obvious improvement in photocatalytic performance. The novel idea to use the precursor sample instead of the synthesized final product may be applied in other fields to increase the required performances.
Tongamp et al.10,11 first reported a solvent-free mechanochemical method (two-step milling: dry milling followed by wet milling) to synthesize Mg–Al LDH. Subsequently, other types of LDH were fabricated.12 Qu et al.13–15 synthesized Ca–Al LDH, Li–Al LDH and tetraborate pillared Li–Al via the two-step milling method and Ferencz et al.16,17 prepared Ca–Fe and Ca–Sn LDH in the same manner. The reported mechanochemical approach based on solid state reaction exhibits some obvious advantages such as no need for heating treatment and no discharge of waste water as in the traditional hydrothermal process. Recently improvements in the adsorption of target pollutants were observed with the mechanochemically prepared LDH products. The dry milling sample, which is known as the precursor, was found to be an excellent anion adsorbent toward anion organic or inorganic pollutants in our recently published works. Wang et al.18 compared the MO adsorption performance of the precursor of Mg–Al LDH, which was prepared by the dry milling of magnesium hydroxide and aluminum hydroxide, with that of well-crystallized Mg–Al LDH products and found that the precursor showed an obviously higher adsorption capacity toward MO. The precursor of ettringite, which was prepared by the dry milling of dihydrate calcium sulfate, calcium hydroxide and aluminum hydroxide, also possessed a much higher adsorption capacity toward phosphate than that of ettringite.19 However, the abovementioned work is limited to the area of anion adsorption. Thus, more work is needed to broaden the application of mechanochemically prepared precursors.
Close contact between the photocatalyst and the organic pollutant is essential for the photocatalytic reaction, which is believed to have a massive impact on the photocatalytic efficiency. Extensive research has been conducted to enhance the access of photocatalysts to target pollutants, whether by increasing the specific surface area of the photocatalyst or dispersing the photocatalyst in porous supporting materials such as diatomite.3,20 However, such elaborate efforts usually increase the production cost, therefore it is difficult to use these materials to purify contaminated water.
Our recent work18 proved that the precursor of Mg–Al LDH prepared by ball-milling exhibits a much higher adsorption capacity than that of the synthesized adsorbent which was mainly realized by surface adsorption. Herein, based on our recently reported phenomenon that the precursor exhibits much higher adsorption capacity than the synthesized adsorbent, we prepare an amorphous photocatalyst (the precursor of Zn–Al LDH) by simply dry-milling Zn4CO3(OH)6·H2O and Al(OH)3 to introduce further photocatalytic activity besides the enhanced adsorption performance. The precursor is found to show much better adsorption and photocatalytic performance toward MO than the well-crystallized Zn–Al LDH, which indicates that the precursor may achieve both easy access to the target by adsorption and decoloration by catalysis. It is believed that such easily prepared precursor meets both the requirements of low cost and high performance and would contribute to the purification of waste water. As a reference experiment, the cationic organic molecule rhodamine B (RHB), which cannot be adsorbed by the LDH, is also used to compare the photocatalytic actions between the precursor and Zn–Al LDH samples.
A two-step operation was used for the synthesis of the precursor and Zn–Al LDH. In the first dry grinding process, 2 g of basic zinc carbonate and Al(OH)3 (Zn/Al molar ratio of 2/1) mixture was ground on a planetary ball mill for two hours at 600 rpm to obtain the precursor. In the second agitation step, 1 g of the precursor was put into a capped Erlenmeyer flask filled with 100 mL of distilled water and stirred for 4 hours on a magnetic stirring apparatus (524G, Meiyingpu, China) at 1200 rpm to fabricate Zn–Al LDH.
Fig. 1 XRD patterns of the raw materials mixture, precursor (prepared by dry milling of raw materials at 600 rpm) and Zn–Al LDH (fabricated by agitating the precursor in water). |
To show the microstructure of the precursor and LDH, the SEM photographs of the precursor and Zn–Al LDH are displayed in Fig. 2. The particles in the precursor sample formed large thick-massive agglomerates without an evident layered structure. When the precursor was agitated in water to prepare the LDH sample, a sheet structure was observed. The agitation operation helped the grain growth of crystalline Zn–Al LDH. In this work, we evaluated the adsorption as well as the photocatalytic performance of the Zn–Al LDH precursor toward MO. The Zn–Al LDH prepared by grinding and agitation operation here was also studied under the same conditions for comparison.
The excellent adsorption performances of the Mg–Al LDH precursor18 and ettringite precursor19 were reported in our previous papers. In this work, the precursor of Zn–Al LDH also shows outstanding adsorption efficiency toward MO. Fig. 3 exhibits the adsorption kinetic experiment (left) and adsorption isotherm experiment (right) results of the precursor and Zn–Al LDH toward MO. The Zn–Al LDH displays a lower removal rate (43.69%) than that of the precursor (96.25%) toward MO after 120 min stirring. The adsorption isotherm experiment results show that the adsorption capacity of the precursor could reach about 250 mg g−1, which is nearly the double that of the Zn–Al LDH (132 mg g−1) toward MO. The Langmuir isotherm, which is assumed to undergo monolayer type coverage of the sorbent on an adsorbent surface,21 was used to describe the obtained data of adsorption isotherm experiments as shown by the red line in Fig. 3. Eqn (1) represents the Langmuir isotherm model.
(1) |
The adsorption kinetic experiment data were processed as pseudo-first order and pseudo-second order and the results are presented in Table 1. The rate constant of the precursor was higher than that of the LDH which indicates a higher adsorption rate for the removal of MO by the precursor. Furthermore, the pseudo-second order model was found to fit better with the correlation coefficient R2 of 0.9961 and 0.9441 for the precursor and LDH, respectively, which are higher than that of the pseudo-first order model. The adsorption rate-determining steps for MO removal by the precursor and LDH were believed to be chemical absorption.
Model | Pseudo-first order | Pseudo-second order | ||||
---|---|---|---|---|---|---|
Parameters | k1 | R2 | qe (mg g−1) | k2 | R2 | qe (mg g−1) |
a Where, k1 and k2 are the rate constants, qt is the amount of solute adsorbed on the adsorbent at time t, and qe is the amount at equilibrium. | ||||||
Precursor | 0.2406 | 0.9729 | 114.3019 | 0.0038 | 0.9961 | 120.4404 |
LDH | 0.1102 | 0.8779 | 46.9974 | 0.0029 | 0.9441 | 52.4855 |
Zn–Al has been demonstrated to be an excellent photocatalyst for the degradation of organic pollutants.7,23 In this work, more attention is paid not only to the adsorption property but also the photocatalytic performance of the precursor toward MO.
The contact area between a photocatalyst and organic pollutants is believed to have a massive impact on its photocatalytic efficiency. A higher contact area often results in a better photocatalytic performance.3,20 The adsorption experiments demonstrate that the precursor could adsorb more MO molecules into its structure, or in other words, the precursor provides a higher contact area for the MO molecules which might promote the photocatalytic decoloration efficiency. To confirm this assumption, the photocatalytic performance of the precursor and LDH for the decoloration of MO solution was determined and the results are displayed in Fig. 5.
Fig. 4 exhibits the experimental data of the photocatalytic decoloration of MO (initial concentration 100 ppm) in aqueous solution by the precursor and as-prepared Zn–Al LDH and the comparison in the remaining MO concentrations by the precursor (A1 with irradiation and A2 without irradiation) and the LDH (B1 with irradiation and B2 without irradiation). The precursor could remove MO up to almost 100% under irradiation, whereas the LDH sample reached a removal rate of only 63% under the same conditions. A better adsorption performance of the precursor toward MO without light irradiation was also observed with an 84% removal rate for the precursor and 56% for the LDH, where a similar improvement in adsorption capacity by the precursor to that of the synthesized LDH was reported for the Mg–Al LDH sample.18
Although a further decrease in the remaining MO concentrations after the treatment of light irradiation to the adsorption operation was observed on both the precursor and LDH samples, a larger decrease by 15.23 mg L−1 was observed with the precursor than that of the LDH sample by 7.10 mg L−1, which indicates higher photocatalytic activity by the precursor sample. It is understood that it is more difficult for the photocatalyst to degrade pollutants at low concentrations. The precursor realized enhanced photocatalytic performance in a relatively low concentration of MO which also proves the improvement in photochemical catalytic ability. For a clear description of the photocatalytic decoloration results, a pseudo-first order model was used to fit the kinetic curve of the MO photocatalytic decoloration, as shown in Table 2. High correlation coefficient R2 values were obtained, which indicates that the pseudo-first-order model well explains the kinetic curve of MO photocatalytic decoloration. The highest rate constant was observed for the photocatalytic decoloration of MO by the precursor, which indicates the highest reaction rate. The simulated qe was 121.33 mg L−1 and 102.05 mg L−1 with a gap of 18.83 mg L−1 for the precursor with or without irradiation, respectively, whereas the gap for LDH with or without light was 4.88 mg L−1 which is much less than that of the precursor. Both the experimental and simulated data prove the enhanced photocatalytic performance of the precursor for the photocatalytic decoloration of MO. We believe that the improvement in photocatalytic activity might result from the physically closer contact of the MO to the adsorbent, as confirmed by the higher removal efficiency in the adsorption section. This simply prepared precursor in a state of massive agglomeration demonstrates better adsorption for MO molecules when dispersed in MO solution, and decomposes the adsorbed MO compositions much more easily when irradiated under ultraviolet light. Thus, the precursor sample exhibits good performances for both adsorption and catalysis.
Parameter | Pseudo-first order qt = qe(1 − e−kt) | ||
---|---|---|---|
k | R2 | qe | |
a Where, k1 is the rate constant, qt is the amount of solute adsorbed on the adsorbent at time t, and qe is the amount at equilibrium. | |||
Precursor with light | 4.5620 | 0.9959 | 121.3376 |
Precursor without light | 3.4225 | 0.9914 | 102.0477 |
LDH with light | 2.5042 | 0.9647 | 73.7035 |
LDH without light | 1.2396 | 0.9893 | 68.8201 |
Fig. 5 shows the XRD patterns of LDH, L-MO-LDH (LDH sample with MO adsorption) and P-MO-LDH (the precursor sample with MO adsorption). New peaks at d003 = 2.5 nm and d006 = 1.24 nm were observed in both L-MO-LDH and P-MO-LDH which could be attributed to the phase of MO intercalated LDH.26 The peak intensity represents the content of the corresponding material. To compare the relative amount of MO intercalated LDH in the L-MO-LDH and P-MO-LDH samples, eqn (2) was applied.
(2) |
Fig. 5 XRD patterns (left) of LDH, L-MO-LDH (LDH sample with MO adsorption) and P-MO-LDH (the precursor sample with MO adsorption) and the adsorption model (right) of the precursor and LDH. |
Besides the XRD characterization with the typical appearances of MO intercalated LDH, IR analysis is another effective way to describe the MO intercalation reaction of Zn–Al LDH. Fig. 6 displays the FT-IR spectra of LDH, P-MO-LDH, L-MO-LDH and MO. The LDH sample shows the typical FT-IR spectrum of Zn–Al–CO3 LDH,27 in which the broad absorption band at 3461 cm−1 is due to the O–H stretching of the hydroxyl groups. The peaks below 1000 cm−1 are attributed to the lattice vibration bands of M–O (M = Zn and Al). The peaks at 1364 cm−1, 1492 cm−1 and 1620 cm−1 result from the asymmetric stretching vibrations of the interlayer carbonate anions, the ν3 vibrations of the carbonate and the infrared bands of free water, respectively. After MO adsorption, the typical infrared bands of the MO molecule such as 1606 cm−1 (NN stretching) and 1119 cm−1 (the vibrations of –SO3) are clearly observed in the spectra of P-MO-LDH (1609 cm−1 and 1122 cm−1, respectively) and L-MO-LDH (1609 cm−1 and 1123 cm−1, respectively) as shown by the dashed box in Fig. 7. The transmittance of the bands is a reflection of the corresponding material content in the sample. It is observed that the transmittance of the peaks at around 1609 cm−1 (NN stretching) and 1122 cm−1 (the vibrations of –SO3) is lower for P-MO-LDH than that of L-MO-LDH, which indicates more MO molecules exist in P-MO-LDH and is consistent with the results in Fig. 5.
Fig. 7 UV-vis adsorption spectra (left) and plots of (Ahν)2 vs. hν (right) for the raw materials mixture, precursor and LDH samples. |
From the results in Fig. 5 and 6, it can be concluded that two mechanisms contributed to the enhanced adsorption activity of the precursor: the disorderly precursor could provide more adsorption sites than the closed structure of Zn–Al LDH for MO removal and the precursor could intercalate more MO molecules into the gallery space of LDH than that of the Zn–Al LDH.
Ahν = K(hν − Eg)n/2 | (3) |
We reported that the co-grinding of raw materials to produce an amorphous precursor is essential for its adsorption properties in our previously published work on the precursor of Ca–Al for Cr(VI) removal.30 The co-existence of the raw materials or simply mixed separately milled materials showed no obvious adsorption behavior for anionic pollutants. Combining the results of the UV-vis adsorption spectra and band gaps of the prepared samples, it can be concluded that dry milling induced a chemical reaction between the raw materials, forming the basic structure of Zn–Al LDH which enhanced the photocatalytic action for MO molecules.
Close contact between the photocatalyst and the organic pollutant is essential for the photocatalytic reaction. Increasing the specific surface area of the photocatalyst or dispersing the photocatalyst in porous supporting materials provides a higher contact area for the photocatalyst to decompose organic pollutants.20 In this precursor system, the enhanced photocatalytic activity of the precursor also from the high contact area of the photocatalyst. It has been proven that the precursor could provide more adsorption sites for MO molecules and intercalate more MO molecules into its gallery space. In other words, the contact area between the precursor and MO molecules was definitely higher than that of the LDH.
Fig. 8 displays the XRD patterns of the precursor and LDH samples dispersed in MO solution with or without irradiation. Without light irradiation, in the patterns of both samples, besides the peaks of Zn–Al LDH phases, new peaks at d003 = 2.5 nm and d006 = 1.24 nm are observed which could be attributed to the phase of MO intercalated LDH.23 The peak intensity of MO intercalated LDH from the precursor sample is much higher than that from the LDH sample, which confirms the higher adsorption of MO. With light irradiation, the peaks of MO intercalated LDH from the LDH sample disappeared completely and became much lower for the precursor sample. As is well known, the photocatalytic reaction degrades organic molecules on the surface of photocatalysts such as TiO2.31 In the case of LDH, the photocatalytic activity sites came from the layered sheets of the LDH. The catalytic sites in the internal space might not work well if the organic pollutant is just adsorbed on the surface, which is quite a long distance from the activity sites. MO intercalation makes it possible for the efficient use of catalytic sites in the internal space as well as that on the surface. In other words, the contact area between the photocatalyst and organic pollutants could be increased when a intercalation reaction takes place. The results in Fig. 8 demonstrate that the photocatalytic properties of LDH came from the sheets of the Zn–Al LDH and intercalated MO molecules were decomposed in the gallery space, as the photocatalytic model shows in Fig. 8. The precursor could intercalate more MO molecules into the layered space of LDH to contact with the sheets of the LDH, which means a higher contact area between MO and the precursor, resulting in the higher photocatalytic efficiency of the precursor.
Fig. 8 XRD patterns (left) of the used samples for the removal of MO with or without irradiation and the photocatalytic model (right) of the precursor and LDH. |
Many previous works have established and discussed the photocatalytic activities of Zn type LDH.32,33 Zn–Al LDH could produce two main intermediate active species (superoxide O2˙− and hydroxyl radicals OH˙) under irradiation for the photocatalytic decoloration of MO. Clear evidence29,33 has proven that O2˙− plays the main role in the initiation of the photocatalytic process in LDH photocatalytic systems.
The LDH samples are well known anionic absorbents, which exhibit high capacity toward anionic organic samples such as MO in this work. On the other hand, very low adsorption capacity was observed with the cationic reagent RHB. To verify our assumption that the excellent adsorption performance of the precursor contributes to the enhanced photocatalytic activity, the photocatalytic decoloration of RHB (initial concentration 4 ppm) by the precursor and as-prepared Zn–Al LDH, in which no adsorption process was involved, was conducted as a reference experiment, and the results are shown in Fig. 9. Without light irradiation, no obvious changes in the remaining RHB concentration were observed on both the precursor and Zn–Al LDH samples, which confirm that they have no adsorption ability toward RHB. Under irradiation, both samples exhibited photocatalytic activity toward RHB and higher efficiency was obtained by the LDH sample than the precursor. Without the adsorption action in this case, it was reasonable to obtain higher photocatalytic efficiency by using the Zn–Al LDH than the precursor sample due to the much better crystallinity, dispersion state and light adsorption of the Zn–Al LDH, as shown in Fig. 1, 2 and 4. These results from RHB reflect that in the case of the precursor to the MO, there exists a synergistic effect of both adsorption and photocatalytic action to enhance the removal efficiency, which is as high as close to complete decoloration.
The data from both MO and RHB confirm the photocatalytic action of the precursor and Zn–Al LDH samples prepared via a simple milling operation. The precursor sample shows enhanced adsorption and photocatalytic activity compared to that of the Zn–Al LDH sample toward MO. The disordered precursor provides more adsorption sites and intercalates more MO molecules into the gallery space of LDH than the closed structure of Zn–Al LDH for MO removal. Thus, a high contact area between the precursor and MO was obtained which resulted in enhanced adsorption and photocatalytic activity. The efficient MO removal almost to complete decoloration particularly on the precursor sample at a relatively high concentration confirms that this method could produce photocatalysts with a high performance at a low cost. Another obvious advantage is that hydroxides and carbonates, which are stable, cheap and easily available compared with the soluble nitrate or sulfate salts of zinc and aluminium used by the co-precipitation method, are directly used as starting samples to prepare the products without emission of other impurities and wastewater. We believe that the precursor prepared by this method could be applied as photocatalyst and would contribute to real wastewater treatment due its overall super performance as a result of the synergistic effect of its adsorption and catalysis capacity.
This journal is © The Royal Society of Chemistry 2017 |