High electrostrictive properties and energy storage performances with excellent thermal stability in Nb-doped Bi0.5Na0.5TiO3-based ceramics†
Received
29th May 2019
, Accepted 1st July 2019
First published on 10th July 2019
Abstract
As a promising candidate material replacing Pb(ZrTi)O3 (PZT), the lead-free Bi0.5Na0.5TiO3 (BNT) system exhibits outstanding piezoelectric and ferroelectric properties. However, the weak thermal stability of these electric properties hampers its practical applications. In this work, we designed and prepared novel Nb-doped 0.76Bi0.5Na0.5TiO3–0.24Bi0.5K0.5TiO3 (BNT–BKT) ceramics with superior temperature stability of electric properties. Both strain as well as discharging properties of 5% Nb-doped BNT–BKT ceramics varied less than 3% and 12.5% respectively from room temperature to 160 °C, ascribed to the enlarged gap between the depolarized temperature (Td or TF–R) and the maximum dielectric temperature (Tm). In addition, we investigated the impacts of Nb doping on the phase transition, dielectric, piezoelectric and ferroelectric behaviors of BNT–BKT ceramics in detail. Temperature dependent dielectric spectrums indicated that Td decreased below room temperature with Nb modifying, revealing that the phase structure transformed from ferroelectric into ergodic relaxor. Accordingly, the maximum strain value of 0.21% and recoverable energy storage of 1.2 J cm−3 were simultaneously acquired at the critical composition of 5% Nb incorporation. Our results provide an effective means of obtaining BNT-based ceramics with simultaneously thermally stable strain and discharge properties for wide temperature actuator and capacitor applications.
1. Introduction
Over the past decades, lead-based ceramics such as PbMg1/3Nb2/3O3-PbTiO3 (PMN-PT), Pb(ZrTi)O3 (PZT) systems were widely investigated in applications of various electromechanical devices owing to their preeminent electric properties.1,2 However, taking into account the irreversible ecological harm caused by lead containing components, developing lead-free materials with alternative properties has inspired much efforts. In recent years, because of their high Curie temperature (320 °C) as well as large spontaneous polarization (∼38 μm C−1),3 Bi0.5Na0.5TiO3 (BNT) ceramics with superior electromechanical performances have received widespread attention. Nevertheless, the high loss and large coercive field (Ec) due to the vaporization of the Bi element result in impaired electric properties of BNT-based ceramics, hampering their practical applications.4
A number of binary systems were designed to improve the electric performances of BNT ceramics, for instance, Bi0.5Na0.5TiO3–Bi0.5K0.5TiO3 (BNT–BKT), Bi0.5Na0.5TiO3–BaTiO3 (BNT–BT) and Bi0.5Na0.5TiO3–K0.5Na0.5NbO3 (BNT–KNN), etc.5 Among these binary components, BNT–BKT systems demonstrate prominent piezoelectric performances with comprehensive superior electric field-induced strain (EFIS) and piezoelectric constant (d33).6 Especially, Tan et al.7 obtained giant strain value of 0.7% in ((Bi1/2(Na0.84K0.16)1/2)0.96Sr0.04)(Ti1−xNbx)O3 ceramics at ambient temperature. Moreover, due to its intrinsic large saturated polarization, the BNT–BKT systems also provide great potential in the applications of energy storage fields.8 Nevertheless, despite aforementioned competitive properties at room temperature, these performances will dramatically deteriorate when the temperature increases, unacceptable for realistic industrial applications and further restricting its development process. Up to now, the thermal stability of BNT-based ceramics is generally poor, and scarcely any attention has been focused on the weak thermal stability of them.9
For the past few years, several approaches had been done to improve the piezoelectric thermal stability of BNT-based ceramics through raising the depolarized temperature (Td) to a higher level to form an enlarged temperature range between RT and Td, such as 0–3-type composites,10 hot-pressed sintering (HPS),11 and quenching process,12 etc. The increased Td improves the thermal stability of piezoelectricity and applies the BNT-based devices to high temperature accelerometers. With the rapid developments of actuators and capacitors recently, the requirements to enhance the thermal stability of strain and energy storage properties are also extremely urgent. Inspired by the strategy of raising the Td to enhance the thermal stability of piezoelectricity mentioned above, lowering the Td could enlarge the temperature range between Td and Tm of strain performances and consequently contribute to the thermal stability of the strain properties. Lately, a great many studies demonstrated that Nb doping in BNT system could effectively break the long-range order, changing the nonergodic polar nanoregions (PNRs) into ergodic ones.13 Furthermore, the addition of Nb would decrease the Td below room temperature while maintain the maximum dielectric temperature (Tm), resulting to the extended temperature range between Td and Tm.14 In addition, a dielectric plateau would form with the increase of Nb content, conducive to the thermal stability of energy storage properties. Therefore, simultaneously thermally stable strain and energy storage behaviors are expected to be obtained in Nb-doped BNT-based ceramics.
In this work, novel Nb-doped 0.76BNT–0.24BKT binary solutions were prepared. The microstructure, dielectric, piezoelectric and ferroelectric properties were studied in detail. The maximum value of strain of 0.21% and energy storage density of 1.2 J cm−3 were simultaneously acquired at 5% doped BNT–BKT ceramics. To evaluate its thermal stability specifically, temperature-dependent strain and discharging properties were also investigated for actual application assessment. The results demonstrate that the strain and discharging properties vary below 3% and 12.5% respectively between 20 and 160 °C at 5% Nb doped BNT–BKT component, demonstrating its appropriate industrial applications in high temperature conditions.
2. Experimental procedure
The 0.76BNT-0.24BKT + xNb (x = 1%, 3%, 5%, 7%, abbreviated as 1Nb, 3Nb, 5Nb, 7Nb, respectively) ceramics were fabricated through solid-state reaction method. Weighed according to the stoichiometry, powders of reagent-grade Bi2O3 (99.99%), Na2CO3 (99.00%), TiO2 (99.80%), K2CO3 (99.99%), Nb2O5 (99.38%) were mixed with agate media and anhydrous ethanol followed by ball-milling for 24 h. Subsequently, the powders were calcined at 850 °C in an air environment. The calcined powders needed ball-milling for 24 h one more time for the sake of the fine particle size. After that, the polyvinyl alcohol PVA was added as binder for granulation. Disks of 13 mm in diameter and 2 mm in thickness were prepared through uniaxial pressing under 150 MPa. After burning out the binder at 750 °C, the samples were sintered at 1150–1200 °C for 2 h in an air atmosphere. In order to avoid the volatile elements of Na, Bi and K, the ceramics were buried in the corresponding powders in the sintering process. For the purpose of electric measurements, circular silver electrodes were coated on both sides of the polished samples.
X-ray diffraction (XRD, D/MAX-2550V; Rigaku, Tokyo, Japan) was utilized to analyze the phase structure of the ceramics. Micrographs of the polished and thermal etched surface was observed by scanning electron microscope (FESEM, Magellan400, FEI Company). Energy dispersive spectrometer (EDS) analysis was gathered from the attachment of the FESEM. The temperature dependence dielectric constant and tangent loss were tested by Hewlett Packard LCR meter. The polarization-electric hysteresis (P–E) loops, current-electric (I–E) loops as well as the strain curves are measured using a ferroelectric measurement system (aixACCT TF Analyzer 2000, Aachen, Germany). The charging–discharging properties were tested by a designed RC load circles.
3. Results and discussion
3.1 Phase formation and microstructure
Fig. 1a displays the XRD patterns of xNb ceramics at room temperature. As shown, the ceramics exhibit pure perovskite structure without any secondary phases when x ≤ 5%. However, with further increase of Nb content to x = 7%, the impurity phase K2Ti6O13 (PDF#40-0403) is obviously observed as indexed in Fig. S1,† demonstrating the solid solution limit of 5%. Fig. 1b and (c) display the enlarged (111) and (200) peaks around 40° and 46°, it can be observed that these two reflection peaks shift to lower angles, consistent with the larger Nb5+ ions replacing the Ti4+ ions with smaller radius [Ti4+(0.604 Å, CN = 6), Nb5+(0.64 Å, CN = 6)] at B-sites.15 The phase structure of the ceramics transforms from P4mm at 1Nb ceramics to pseudocubic structure with higher Nb content, evidenced from the fact that the (200)/(002) peaks merge into a single (200)pc peak.16
|
| Fig. 1 (a) XRD patterns of xNb ceramics. (b and c) Enlarged (111) and (200) peaks around 40° and 46°, respectively. | |
Fig. 2 display the SEM images of the polished and thermal-etched surface. The samples exhibit homogeneous and dense microstructures for compositions up to x = 5%. The secondary phase obviously appears with the further increase of Nb content to x = 7%. The results of the element spot scanning measured by EDS demonstrate that the secondary phase is Bi and Na deficient and K enriched phase, as shown in Fig. S2† and Table S1,† which is consistent with the K2Ti6O13 phase determined by XRD. In addition, the average grain size doesn't display significant composition dependence with the similar average grain size ∼2.3 μm measured through linear intercept method. The independence between composition and grain size indicates that the variation of strain and energy storage properties have no relation to the size of grain.
|
| Fig. 2 The scanning electron microscopy photographs of xNb doped BNT–BKT ceramics with (a) x = 1%, (b) x = 3%, (c) x = 5%, (d) x = 7%. | |
3.2 Dielectric properties
Fig. 3 presents the temperature dependence of dielectric constant (ε) and loss (tanδ) for poled ceramics under varied frequencies. Three significant dielectric abnormal peaks appear at TF–R, Ts and Tm. The TF–R (equal to the depolarized temperature Td) reflects the ferroelectric to relaxor transition temperature, indicating that the ferroelectric P4mm domains change into relaxor P4bm polar nanodomains (PNRs) during heating. However, no TF–R could be found in the dielectric curves when x ≥ 3%, indicating that the TF–R is below room temperature and the ceramics have changed into the relaxor phase with p4bm nanodomains at room temperature.17 The difference of phase structure obtained from XRD and ε–T curves is ascribed to the fact that the nanoscale structure could not detected by XRD accurately.18 These nanodomains would grow into ferroelectric domains under electric field, conductive to large strain and energy storage properties. The Ts, which is related to the thermal evolution of tetragonal PNRs, also decreases with increase of the Nb content. It's noteworthy that the ε merges immediately as the temperature increase above Ts, revealing the disappearance of relaxor characteristics as well as the relation between Ts and the relaxor behavior in this system. With the temperature further increasing, the maximum dielectric constant εm appears at around 280 °C, which is usually defined as Tm (Tc). The barely changed Tm accompanied by notably decreased TF–R results in the widened gap between TF–R and Tm, as shown in Fig. 4. Furthermore, with the increasing Nb content, the dielectric constant maximum εm decreases sharply, getting closer to the dielectric constant value at Ts and resulting in the formation of dielectric plateau in a wide temperature range.19 The temperature independence of the dielectric properties is closely related to the thermal stability of electric behaviors.19
|
| Fig. 3 Temperature dependent dielectric curves of xNb ceramics for (a) x = 1%, (b) x = 3%, (c) x = 5%, (d) x = 7% component. | |
|
| Fig. 4 Phase diagram of xNb ceramics. | |
3.3 Electrostrain properties
Fig. 5a exhibits the bipolar strain behaviors of xNb ceramics under 5 kV mm−1 and 10 Hz. The 1Nb ceramics exhibit typical butterfly-shaped bipolar S–E curves with a positive strain (Spos) of 0.12% and negative strain (Sneg) of 0.1%, which is the characteristic of ferroelectrics as the negative strain is related to the domain back switching during loading electric field.20 With the increase of Nb content, it could be clearly observed that the Sneg has been declining to 0 while the Spos rises significantly. As illustrated in Fig. 5b, the Spos and Sneg value reach the maximum of 0.19% and the minimum of 0 respectively at 5Nb ceramics. As the Nb content reaches 7%, the Spos value drops to 0.12% and Sneg value remains 0. The decrease of Sneg is related to the reduction of the domain wall density induced by the Nb modifying, while the ultimate vanishment of which indicates that Nb-doped BNKT ceramics have changed into the ergodic relaxor ferroelectrics, in good agreement with dielectric curves.
|
| Fig. 5 The component dependent (a) bipolar strain and (c) unipolar strain curves of xNb ceramics under 5 kV mm−1. (b) The evolution of component dependent Sneg and Spos. (d) The component dependent piezoelectric constant d33 and normalized strain . | |
To assess the suitability of the designed ceramics in actuator applications, unipolar strain curves are depicted in Fig. 5c. On increasing the Nb content from 1% to 5%, the strain value increases from 0.10% to 0.21%, and decreases subsequently to 0.11% at x = 7%. To better explain the physical mechanism of the strain, the d33 as well as normalized strain Smax/Emax () of the xNb ceramics were measured and analyzed, as shown in Fig. 5d. The BNKT ceramics exhibit large d33 of 180 pC/N, in proximity with its of 200 pm V−1, indicating that the strain value of 1Nb ceramics mainly origins from the converse piezoelectric effect. With the increase of Nb doping, the d33 keeps reducing until nearly 0 pC/N at 7Nb ceramics while the increases sharply reaching the maximum value of 420 pm V−1 at x = 5%, and eventually it reduces to 200 pm V−1 at x = 7%. This phenomenon reveals that the strain property mainly origins from the electric field induced relaxor and ferroelectric phase transition because of their low energy barrier.21 The decrease of strain at x = 7% is caused by the enlarged energy barrier of the phase transition.
For the purpose of evaluating the thermal stability of the strain behavior, temperature dependent unipolar strain curves of the 5Nb component are characterized. As depicted in Fig. 6a, the 5Nb ceramics possess excellent thermal stability of the strain behavior, almost maintaining the fixed value in the measured temperature region of 20–160 °C with the variation less than 3%. The excellent thermal stability of this strain property is much superior than many other systems,22–25 as displayed in Fig. 7. The excellent temperature independence of strain value of our 5Nb ceramics demonstrates its advantages in practical applications of actuators. Meanwhile, as shown in Fig. 6b, the strain hysteresis of these unipolar curves decreases sharply from 24% to 0 with the temperature increasing. It is worth noting that the strain value maintains a high level near Ts while the hysteresis is zero. This is an interesting phenomenon, because if the subsequent work can adjust the Ts to room temperature, the BNT-based ceramics with both high strain and ultra-low hysteresis can be obtained, which has great application prospects.
|
| Fig. 6 The temperature dependent (a) the strain value of 5Nb ceramics and (b) the corresponding hysteresis. | |
|
| Fig. 7 Comparison of the temperature dependence of the as normalized to the for various systems. | |
3.4 Energy storage properties
To characterize the energy storage performances of the ceramics, P–E loops under critical electric field of 12 kV mm−1 of different content of Nb are displayed in Fig. 8. The 1% Nb modified BNKT ceramics exhibit typical saturated ferroelectric performance with both large Pm and Pr of 48 μC cm−2 and 40 μC cm−2 respectively, corresponding to its butterfly-shaped strain curves. With the Nb content increasing to 5%, the Pr reduces dramatically accompanied by the decline of Pm, resulting in the pinched P–E loops. The obvious changes of P–E loops confirm that the long-range ferroelectric order of BNKT ceramics has been disrupted into ergodic relaxor (ER) phase.26 As the Nb content further increases to 7%, the critical electric field for the phase transition between relaxor and ferroelectric increases sharply, evidenced by the quasi-linear loops with relatively low Pm. Fig. 8b presents the corresponding current-electric field (I–E) loops. As is displayed, the 1% doped BNKT ceramics show typical ferroelectric I–E curves with two sharp current switching peaks. The inherent ferroelectric order exists stably even when the electric field is withdrawn, manifested in the large Pr. On increasing the Nb content to 3%, four current peaks (P1, P2, P3, P4) appear,6,26 it's reported that these four current peaks are related to the ER phase induced by the Nb content modifying. The ER phase would transform into metastable ferroelectric phase under exerted electric field, corresponding to P1/P3 current peaks, resulting in large Pm. When removing the electric field, the induced long-range order would change back to the initial ER state, corresponding to P2/P4 current peaks, resulting in the low Pr. Both large Pm and low Pr are beneficial to acquire high energy storage property. According to the formula:18,27,28 |
| (1) |
|
| (2) |
|
| (3) |
Where P, Pm, Pr, and E indicate the polarization, maximum polarization, remnant polarization, and exerted electric field, respectively. Pm and Pr play important role in improving the value of Wrec. Thus we summarized the Pm, Pr and ΔP (Pm − Pr) in Fig. 8c. When increasing Nb content from 1% to 7%, Pm smoothly decreases from 48 μC cm−2 to 27 μC cm−2 while Pr sharply reduces from 40 μC cm−2 to 3 μC cm−2. As a result, the ΔP achieves the maximum value of 32 μC cm−2 at 5Nb ceramics, boosting high Wrec of 1.2 J cm−3 in this component, as shown in Fig. 8d. In addition, the η value keeps increasing until x = 7%, ascribed to the reduced hysteresis of P–E loops.
|
| Fig. 8 (a) P–E loops of xNb ceramics and (b) corresponding I–E curves at room temperature. (c) The component dependent Pm, Pr and ΔP (Pm − Pr). (d) The component dependent calculated energy storage density and efficiency. | |
3.5 Charging–discharging properties
To assess the temperature stability of the 5Nb ceramics, temperature dependent P–E loops at 8 kV mm−1 are depicted in Fig. 9a. The ferroelectric properties exhibit stable trend with the polarization value (Pm and Pr) exhibiting little changes in the measured temperature range from 20 to 160 °C, as displayed in the inset of Fig. 9a. To evaluate the practical application performances, temperature dependent overdamped discharge current curves of the 5Nb ceramics under 8 kV mm−1 are illustrated in Fig. 9b. As shown, the 5Nb ceramics exhibit similar discharging performances under different temperature, with the current curves reaching the maximum value rapidly and lasting less than 1 μs. In the measuring temperature range, the current curves maintain the peak value of 46 A, exhibiting excellent thermal stability. According to the formula , where the R, V denote the total load resistor (200 Ω) and sample volume respectively,29 the calculated Wd–t value are illustrated in Fig. 9c. The t0.9 indicated by the dash line in Fig. 9c means the time required to release 90% of the stored energy (Wd). It's noteworthy that the Wd and t0.9 change from 0.72 J cm−3 and 124.8 ns to 0.81 J cm−3 and 121.6 ns respectively in the range of 20–160 °C, keeping the variation less than 12.5%, as illustrated in Fig. 9d. The superior thermal stability of the 5Nb ceramics demonstrates its great potential in high temperature energy storage applications.
|
| Fig. 9 (a) The temperature dependent P–E loops of 5Nb ceramics at 8 kV mm−1, the inset shows corresponding Wrec and η. (b) Overdamped discharging current curves of the 5Nb ceramis at 8 kV mm−1. (c) The calculated Wd–t curves. (d) The summarized Wd and t0.9 values as a function of temperature. | |
At present, the doping of elements mainly improves the temperature stability of strain or energy storage performances singly, and there are fewer materials simultaneously possessing temperature and energy storage stability. Despite this, our Nb-doped BNT-based ceramics attained superior results in temperature stability in both strain and energy storage performances compared with other currently promising materials, as shown in Table 1.30–35 Therefore, these results provide new strategies for the application researches of BNT-based ceramics.
Table 1 The temperature stability of the investigated materials compared with other perovskite systemsa
Materials |
Strain |
Variation |
Wrec (J cm−3) |
Variation |
Temperature range |
References |
PZT: Pb(Zr0.53Ti0.47)O3 BCZT: (Ba0.85Ca0.15)(Zr0.1Ti0.9)O3 KNN: (K0.48Na0.52)NbO3 SZ: SrZrO3 BNZ: (Bi0.5Na0.5)ZrO3 BNKT: Bi0.5(Na0.84K0.16)0.5TiO3 ST: SrTiO3 BCT: Ba0.8Ca0.2TiO3 BMT: BiMg0.5Ti0.5O3 BZS:Bi(Zn0.5Sn0.5)O3. |
Ho doped BCZT |
∼0.165% |
<2% |
— |
— |
20–70 °C |
30 |
Sb doped KNN-SZ-BNZ |
∼0.14% |
<10% |
— |
— |
20–180 °C |
31 |
Ta doped BNKT-ST |
∼0.35% |
∼46% |
0.52 |
<10% |
25–135 °C, 75–150 °C |
32 |
BNT modified BT |
— |
— |
2.14 |
<12% |
25–175 °C |
33 |
BFO modified BCT-BMT |
— |
— |
0.39 |
∼15% |
25–110 °C |
34 |
BZS modified BT |
— |
— |
∼1.12 |
<15% |
20–160 °C |
35 |
Nb doped BNT-BKT (this work) |
0.21% |
<3% |
1.2 |
<15% |
25–160 °C |
This work |
4. Conclusion
In this work, we designed and prepared Nb modified BNT-based ceramics with excellent thermal stability through simple solid-state reaction method. Enhanced strain and energy storage properties (0.21% and 1.2 J cm−3 respectively) were obtained in 5Nb ceramics due to relaxor and ferroelectric phase transition. The extended temperature range between TF–R and Tm accompanied by wider dielectric plateau jointly contribute to the thermal stability of piezoelectric and discharging behaviors. As a result, the strain and discharge energy density of 5Nb component vary less than 3% and 12.5% respectively in the temperature range of RT and 160 °C. The excellent temperature stability of 5Nb ceramics indicates its outstanding applications in the high temperature conditions of dielectric capacitors and actuators.
Conflicts of interest
There are no conflicts of interest to declare.
Acknowledgements
This work was supported by the National Natural Science Foundation of China (Grant No. 11774366, 51831010) and Natural Science Foundation of Shanghai (Grant No. 18ZR1444900).
References
- J. Rödel, K. G. Webber, R. Dittmer, W. Jo, M. Kimura and D. Damjanovic, J. Eur. Ceram. Soc., 2015, 35, 1659–1681 CrossRef.
- P. Baettig, C. F. Schelle, R. LeSar, U. V. Waghmare and N. A. Spaldin, Chem. Mater., 2005, 17, 1376–1380 CrossRef CAS.
- M. Davies, E. Aksel and J. L. Jones, J. Am. Ceram. Soc., 2011, 94, 1314–1316 CrossRef CAS.
- R. A. Malik, A. Hussain, A. Maqbool, A. Zaman, T. K. Song, W.-J. Kim and M.-H. Kim, J. Alloy. Comp., 2016, 682, 302–310 CrossRef CAS.
- G. Dong, H. Fan, J. Shi, M. Li and W. Jo, J. Am. Ceram. Soc., 2015, 98, 1150–1155 CrossRef CAS.
- X. Zhou, Z. Yan, H. Qi, L. Wang, S. Wang, Y. Wang, C. Jiang, H. Luo and D. Zhang, J. Eur. Ceram. Soc., 2019, 39, 2310–2317 CrossRef CAS.
- X. Liu and X. Tan, Adv. Mater., 2016, 28, 574–578 CrossRef CAS.
- Y. Wu, Y. Fan, N. Liu, P. Peng, M. Zhou, S. Yan, F. Cao, X. Dong and G. Wang, J. Mater. Chem. C, 2019, 7, 6222–6230 RSC.
- L. Jin, W. Luo, L. Wang, Y. Tian, Q. Hu, L. Hou, L. Zhang, X. Lu, H. Du, X. Wei, G. Liu and Y. Yan, J. Eur. Ceram. Soc., 2019, 39, 277–286 CrossRef CAS.
- J. Zhang, Z. Pan, F. F. Guo, W. C. Liu, H. Ning, Y. B. Chen, M. H. Lu, B. Yang, J. Chen, S. T. Zhang, X. Xing, J. Rodel, W. Cao and Y. F. Chen, Nat. Commun., 2015, 6, 6615 CrossRef CAS.
- R. I. Mahdi and W. H. A. Majid, RSC Adv., 2016, 6, 81296–81309 RSC.
- Z.-T. Li, H. Liu, H.-C. Thong, Z. Xu, M.-H. Zhang, J. Yin, J.-F. Li, K. Wang and J. Chen, Adv. Electron. Mater., 2019, 5, 1800756 CrossRef.
- K.-N. Pham, A. Hussain, C. W. Ahn, W. Kim, S. J. Jeong and J.-S. Lee, Mater. Lett., 2010, 64, 2219–2222 CrossRef CAS.
- L. Li, M. Zhu, Q. Wei, M. Zheng, Y. Hou and J. Hao, J. Eur. Ceram. Soc., 2018, 38, 1381–1388 CrossRef CAS.
- R. D. Shannon, Acta Crystallogr., 1976, A32, 751–767 CrossRef CAS.
- F. Li, K. Yang, X. Liu, J. Zou, J. Zhai, B. Shen, P. Li, J. Shen, B. Liu, P. Chen, K. Zhao and H. Zeng, Scripta Mater., 2017, 141, 15–19 CrossRef CAS.
- J. Wu, A. Mahajan, L. Riekehr, H. Zhang, B. Yang, N. Meng, Z. Zhang and H. Yan, Nano Energy, 2018, 50, 723–732 CrossRef CAS.
- W. Huang, Y. Chen, X. Li, G. Wang, N. Liu, S. Li, M. Zhou and X. Dong, Appl. Phys. Lett., 2018, 113, 203902 CrossRef.
- F. Hu, X. Chen, P. Peng, F. Cao, X. Dong and G. Wang, J. Am. Ceram. Soc., 2018, 101, 4434–4440 CrossRef CAS.
- Z. Rashad and A. Feteira, Mater. Lett., 2018, 222, 180–182 CrossRef CAS.
- L. Wang, R. Liang, Z. Zhou and X. Dong, Scripta Mater., 2019, 164, 62–65 CrossRef CAS.
- J. Hao, W. Li, J. Zhai and H. Chen, Mater. Sci. Eng., R, 2019, 135, 1–57 CrossRef.
- L. Jin, J. Qiao, L. Wang, L. Hou, R. Jing, J. Pang, L. Zhang, X. Lu, X. Wei, G. Liu and Y. Yan, J. Alloy. Comp., 2019, 784, 931–938 CrossRef CAS.
- X. Lu, L. Hou, L. Jin, L. Wang, Y. Tian, K. Yu, Q. Hu, L. Zhang and X. Wei, Ceram. Int., 2018, 44, 5492–5499 CrossRef CAS.
- X. Lu, L. Wang, L. Jin, Q. Hu, Y. Tian, L. Hou, K. Yu, L. Zhang, X. Wei, Y. Yan and G. Liu, J. Alloy. Comp., 2018, 753, 558–565 CrossRef CAS.
- N. Liu, R. Liang, Z. Zhou and X. Dong, J. Mater. Chem. C, 2018, 6, 10211–10217 RSC.
- N. Sun, Y. Li, Q. Zhang and X. Hao, J. Mater. Chem. C, 2018, 6, 10693–10703 RSC.
- T. Li, X. Lou, X. Ke, S. Cheng, S. Mi, X. Wang, J. Shi, X. Liu, G. Dong, H. Fan, Y. Wang and X. Tan, Acta Mater., 2017, 128, 337–344 CrossRef CAS.
- F. Li, X. Hou, J. Wang, H. Zeng, B. Shen and J. Zhai, J. Eur. Ceram. Soc., 2019, 39, 2889–2898 CrossRef CAS.
- L. Wang, W. Bai, X. Zhao, F. Wen, L. Li, W. Wu, P. Zheng and J. Zhai, J. Mater. Sci.: Mater. Electron., 2019, 30, 9219–9230 CrossRef CAS.
- X. Lv, J. Wu, J. Zhu and D. Xiao, Phys. Chem. Chem. Phys., 2018, 20, 20149–20159 RSC.
- R. A. Malik, A. Hussain, A. Maqbool, A. Zaman, T. K. Song, W.-J. Kim and M.-H. Kim, J. Alloy. Comp., 2016, 682, 302–310 CrossRef CAS.
- L. Chen, H. Wang, P. Zhao, C. Zhu, Z. Cai, Z. Cen, L. Li and X. Wang, J. Am. Ceram. Soc., 2019, 102, 4178–4187 CrossRef CAS.
- M. Xu, B. Peng, J. Zhu, L. Liu, W. Sun, G. J. T. Leighton, C. Shaw, N. Luo and Q. Zhang, J. Alloy. Comp., 2019, 789, 303–312 CrossRef CAS.
- M. Zhou, R. Liang, Z. Zhou and X. Dong, J. Mater. Chem. C, 2018, 6, 8528–8537 RSC.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra04069b |
|
This journal is © The Royal Society of Chemistry 2019 |
Click here to see how this site uses Cookies. View our privacy policy here.