Anna
Nowik-Zajac
,
Iwona
Zawierucha
and
Cezary
Kozlowski
*
Institute of Chemistry, Health and Food Sciences, Jan Dlugosz University of Czestochowa, PL42200 Czestochowa, Poland. E-mail: c.kozlowski@ajd.edu.pl; a.zajac@ajd.edu.pl
First published on 2nd October 2019
This paper discusses the results of studies on the transport of Ag(I) across polymer inclusion membranes (PIMs), derivatives of calixpyrroles with methyl (KP1) and carboxyl (KP2) groups, as ion carriers, o-nitrophenyl pentyl ether (o-NPPE) as a plasticizer and cellulose triacetate (CTA) as support. The influence of the pH of the source phase, metal concentration, stripping phase as well as carrier and plasticizer concentration on the efficiency of Ag(I) transport through PIM is presented. Long-term experiments with a supported liquid membrane and a plasticizer membrane demonstrate the durability of the studied PIMs. The obtained results indicate that the competitive transport of Cu(II), Zn(II), Ag(I) and Cd(II) from the aqueous nitrate source phase through KP1 and KP2 is an effective separation method for Ag(I) ions. The prepared PIMs were characterized by scanning electron microscopy (SEM), and atomic force microscopy (AFM) techniques.
Up to now various techniques, including chemical precipitation, extraction, ion exchange, membrane separation and sorption, have been developed for the effective removal of metal ions from different aqueous solutions at various concentrations.1
In the process of selective recovery and concentration of metal ions from aqueous solutions liquid membranes, and in recent years also polymer inclusion membranes (PIMs) could be an alternative for liquid–liquid extraction procedures.2 The efficiency and selectivity of PIM depends on the nature of metal ion carrier introduced into membrane. Different metal ions that can be transported from the feed solution to the stripping solution using PIMs containing a number of carriers are listed by Nghiem et al.3 and Almeida et al.4
PIM potential for the separation of metallic species is due to their characteristic high selectivity and mechanical properties, which can be improved. For example reinforcing the membrane's support material with functional nanomaterials improves the permeability, contamination resistance, mechanical and thermal stability of the membranes.5 On the other hand the application of constant electric current in membrane extraction experiments opens a new opportunity for achieving the excellent selectivity and long-term use of polymer inclusion membrane.6
The present commercial extractants enable an efficient removal of metal ions but sometime with low selectivity. Therefore PIM researchers are generally interested in macrocyclic and macromolecular compounds due to their excellent separation selectivity.
The complexation ability of these compounds depends on the size of the ligand cavity, on the ionic potential of the cation to be bound, on the spatial localization of donor binding sites of the ligand, on the presence of additional chemical groups and heteroatoms, and on the nature of the used solvent.
Today a main drawback, strongly limiting the practical use of liquid membranes, constitutes their low durability and nonstable work. These are obviously related with the composition of liquid membranes (the kind of the carrier, of organic solvent and of the surfactant) as well as with their structure.7,8
Lifetime of liquid membranes is limited by washing the carrier from membrane to aqueous solvents, forming an emulsion on the interface membrane, the progressive wettability of the pores of the polymeric support, pressure differences between the source and receiving phases, blocking of the membrane pores by the formation of sediment on the membrane surface as well as by the appearance of an osmotic pressure gradient on both sides of the membrane.9
An important factor determining the possibility of the commercial use of polymer inclusion membranes is the stability of their operation. Although PIMs are considered to be more stable compared to supported liquid membranes (SLM), washing the carrier and plasticizer or modifier (if present) from organic phase filling PIM matrix pores, which resulted in the reduction of examined metal ions separation, was observed under certain conditions of metal ions transport.10–12 The loss of the membrane liquid phase, consisting of the carrier and the plasticizer or modifier (if present), could be minimized by increasing the concentration of common anions in the aqueous solution.13 It should be noted that the much higher stability of PIM (compared to SLM), allows their multiple use.14
The literature data devoted to the transport across PIMs applied for the analysis of pharmaceutical, clinical and environmental samples show that these have good long term stability and can be reused up to 30 times without loss of performance.15–17
The growing, especially in recent years, interest in macrocycles as potential transporters of metal ions and neutral molecules is a result of their easy synthesis from commercially available reagents, high thermal and chemical stability and selective complexation of ions and neutral molecules. Due to the simple synthesis, often with high yields, and efficient functionalization by substituents that modify their complexing properties, calixpyrroles induce recently a great interest as the selectophores of metal ions. This results also from the fact that in many chemical and biochemical processes the binding of ions plays a key role, therefore compounds able to bind ions are intensively studied.18
The demand for highly purified precious metals free from silver contaminations has increased in the electronics industry, which prepares devices using precious metals.19 Moreover, silver as the most useful noble metal finds numerous applications in other fields such as jewellery, photography, anti-corrosive alloys, etc. It is estimated that about 12% of the world's silver resources are used in the production of light-sensitive devices. All over the world, several tons of silver are lost annually in the waste from photographic and galvanizing plants.20 Since in addition to being a precious metal it is toxic, the separation and recovery of silver from industrial effluents is of a paramount importance.21
Nowik-Zajac et al.22 studied the transport of Ag(I) and Cu(II) ions transport across PIMs containing calix[4]pyrrole[2]thiophene as ion carrier and found that the transport Ag(I) ions is faster than Cu(II) ions.
Amiri et al.23,24 showed that the derivatives of the calix[4]pyrroles dissolved in an oil and immobilized on the supported liquid membrane (SLM) based on a polypropylene matrix are effective and selective Ag(I) ion transporters, but do not transport at all Cu(II), Ni (II), Zn(II), Pb(II), Co(II), Cd(II), Cr(III), Fe(II) and Fe(III) ions. The addition of picric acid to the source phase caused shortening of the time of transport process from 3.5 hours25 to 75 minutes.24
The present work deals with the transport of Ag(I) and Cu(II) from nitrate aqueous solutions through PIMs that contain cellulose triacetate or polyvinyl chloride as a support, o-nitrophenyl pentyl ether as a plasticizer and calixpyrrole derivatives as ion carriers. We have tested several parameters, such as the concentration of the carrier, the effect of pH in the acceptor phase, and the nature of stripping agents. We have characterized the membrane with SEM, AFM as well as selectivity and reliability studies.
A surface characterization of the polymer membranes was performed using by Atomic Force Microscopy (AFM) (Digital Instruments Veeco Metrology Group). Pores characterization was performed using the AFM image processing program NanoScope v.720 (Digital Instruments Vecco Metrology Group), which enabled the calculation of parameter: roughness (Ra). The Ra parameter is the standard deviation of the z values within the box cursor and is calculated as:
(1) |
A 5 kV scanning electron microscope (SEM) (Quanta 3D FEG, FEI Company) (Hitachi S4500) was used to analyze membrane morphology. Membrane samples were prepared by freezing under liquid nitrogen (70 K) and rapid fracturing, resulting in a clean break fracture image to view the cross-section. The samples were mounted with conductive glue to metal stubs with the fractured edge up and then coated with gold by sputtering. These samples were then viewed in the SEM at around 50 μm magnification.
The composition of the membranes expressed as a weight percentage for KP1 and KP2 was as follow: 63–69% plasticizer; 30–30% support; 0.05–7% carrier and 57–67% plasticizer; 27–33% support 0.1–16% carrier, respectively.
The aqueous source phase was a 0.00050 M AgNO3 and Cu(NO3)2, the aqueous receiving phase was 0.10 M sodium thiosulfate Na2S2O3 (50 cm3). Transport was conducted at a room temperature (23–25 °C) and both source and receiving aqueous phases were stirred at 600 rpm with synchronous motors. Samples (0.10 cm3) of an aqueous source phase were removed periodically via a sampling port with a syringe and analyzed to determine Ag(I) and Cu(II) concentration.
The source phase acidity was controlled by pH meter (multifunctional pH meter, CX-731 Elmetron, with combine pH electrode, ERH-136, Hydromet, Poland). Kinetics of transport process through polymer inclusion membrane (PIM) is described by a first-order reaction in respect to metal ion concentration:20
ln(c/ci) = −kt | (2) |
To calculate the k value, a plot of ln(c/ci) versus time was prepared. The rate constant value for the duplicate transport experiment with the averaged standard deviation was calculated. The permeability coefficient (P) was calculated as follows:
P = (V/A)k | (3) |
The initial flux (Ji) was determined as equal to:
Ji = Pci | (4) |
To describe the efficiency of metal ion removal from the source phase, the recovery factor (RF) was calculated as:
(5) |
The metal ion concentrations were measured by flame atomic absorption spectrometry (Solar 939, Unicam). The limits of detection for silver and copper of a flame atomic absorption spectrometry method are: 0.02 μg mL−1 and 0.03 μg mL−1, respectively.
The selectivity coefficient S was defined as the ratio of initial fluxes for M1 and M2 metal ions, respectively.
S = Ji,M1/Ji,M2 | (6) |
The reported values correspond to the average of three replicates; the standard deviation observed was within 2%.
The rate of change of concentration of Ag(I) ions in source, receiving phase and the membrane was analyzed for the transport of Ag(I) ions through PIM containing KP2 providing concentration profile of the metal as a function of time.
As seen in Fig. 2, the kinetic curves of c/ci relationship in the function of time are of an exponential nature that confirms the kinetic model of metal ions primary transport proposed by Danesi et al. in relation to the supported liquid membranes (SLM).27
The rate of transport at the border of source phase and membrane, as well as membrane and the receiving phase is comparable, i.e. complexation and decomplexation reactions occur with the same rate. Small saturation of the membrane with Ag(I) – KP1 as well as KP2 complex proves the establishing of quasi-stationary state in the membrane phase.
To determine the repeatability of Ag(I) ions transport measurements through PIM containing KP1 and KP2, each experiment was repeated 5 times.
Average constants of transport process (k) were estimated, based on the slopes of linear relationship ln(c/ci) = f(t) obtained for applied membrane, and the values of initial fluxes of Ag(I) ions from the source phase (Ji) were calculated based on them. The calculation results are presented in Fig. 3. The coefficients of determination (r2) of linear relationships ln(c/ci) in the function of time for KP1 and KP2 carriers amounted to 0.9901 and 0.9115, so the correlations were designated at a high level of significance. Thus, these results are burdened with a relative error not exceeding 1%, and concurrently are calculated at high values of determination coefficients exceeding 0.91. This means that the repeatability of the results of transport through PIM is very good. It can be noticed, taking into account the obtained values of kinetic parameters and their statistical evaluation, that the repeatability of the results is good.
It turned out that the values of initial fluxes of Ag(I) ions transport increase with an increasing pH from 2.0 to 4.0. For pH = 4.0, the maximum initial fluxes of Ag(I) ions transport from the aqueous source phase containing 5 × 10−4 M AgNO3 through PIM amounted to 0.71 μmol m−2 s−1 for KP1, and 1.62 μmol m−2 s−1 for KP2. However, in pH range of 4.0–6.0, the transport flux was stabilized at a constant level. The highest increase of Ag(I) ions transport rate was observed for KP2, which is a carboxyl derivative of calixpyrroles. However, above pH = 4.0, the share of carrier particle deprotonation was smaller, hence, small changes in Ji value were observed for the measurements above pH = 5.0. This indicates cooperative transport mechanism, but with greater participation of complexes formation by incorporation the Ag(I) ions into the cavity of KP2.
Then, an effect of initial AgNO3 concentration in the source phase on the rate of transport through PIM was examined. Four AgNO3 solutions at pH 4.0, containing 1.0 × 10−4 M; 2.5 × 10−4 M; 5.0 × 10−4 M and 1.0 × 10−3 M of this metal ions were prepared and they were used as the source phases, in order to determine the kinetics of PIM process due to the concentration of Ag(I) ions in source phase. The 0.10 M Na2S2O3 solution was used as the receiving phase.
Fig. 5 shows the obtained linear effect of (Ji) value on Ag(I) concentration in the source phase in log–log arrangement.
The change in the values of Ag(I) initial fluxes as a function of metal concentration in the source phase (ci) in a logarithmic arrangement is linear. It indicates that the reactions takes place in the boundary of source phase/membrane involve single Ag(I) cation, therefore, this is the first order reaction in respect of a metal ion.
The literature review shows several applications of liquid membranes to real waste solutions treatment. According to the literature23,28,29 concentration of Ag(I) ions in wastewater was between 4.0–8.0 × 10−4 M. Tarahomi et al.28 showed composition of silver plating and photographic waste solution in which silver concentration was 5 × 10−4 M at pH 3. Amiri et al.23 also showed that the derivatives of the calix[4]pyrroles dissolved in an oil and immobilized to the supported liquid membrane (SLM) based on a polypropylene matrix are effective and selective Ag(I) ion transporters. Concentration of Ag(I) ions was 8.0 × 10−4 M, pH 4. In next experiments, the silver concentration in source aqueous phase was 1 × 10−3 M at pH 4.
Fig. 6 presents the relationship of recovery coefficient (RF) vs. the time of Ag(I) transport through PIM containing KP1 and KP2. 0.10 M Na2S2O3, 0.10 M EDTA as well as 0.10 M CH3COONa aqueous solutions at pH = 6.0 were used as the receiving phases.
In the case of membrane system containing calixpyrrole carriers KP1 and KP2 the transport of silver ions was effectively followed using sodium thiosulfate as aqueous receiving phase.
The maximum value for the Ag(I) recovery factor after 6 hours of transport obtained for KP2 was RF = 74.5% (0.10 M Na2S2O3 as the receiving phase). The yield of Ag(I) ions separation using the above mentioned receiving phases decreased in the following order: Na2S2O3 ≫ CH3COONa > EDTA. Only the use of 0.10 M Na2S2O3 solution leads to effective decomplexation of labile Ag(I) – calixpyrroles complexes in the membrane. The separation of Ag(I) ions from aqueous solutions using CH3COONa and EDTA was low and did not exceed the value RF = 12%. Maming et al.30 also suggests a Na2S2O3 solution as an appropriate receiving phase in the membrane systems used for the selective Ag(I) removal. They demonstrated that PIM containing p-tert-buthylcalix[4]-arene-tetraethyl ester gives the most efficient transport for Ag(I) ions using 0.10 M Na2S2O3 solution as the receiving phase. The recovery factor for Ag(I) ions was 65.9%, then. Amiri et al.23 using 0.15 M Na2S2O3 as the receiving phase determined the rate and efficiency in the transport of Ag(I) ions through PIM containing calix[4]pyrrole. The flux and RF for Ag(I) were found to be equal to 1.57 μmol m−2 s−1, and 38%, respectively.
The carrier concentrations in the membranes expressed as percent by weight were for KP1 0.05–7% and 0.1–16% for KP2.
Each experiment was carried out for 6 hours. The membranes without ion carrier did not transport Ag(I) ions, which indicates that carrier concentration is crucial for the facilitated transport of silver ions through PIM.
The saturation of polymer inclusion membrane with the ion carrier occurs at a concentration equal to 0.10 M (based on plasticizer volume) both for carriers KP1 and KP2. The rate of transport determined for that concentration of the carrier is maximum and reaches 0.71 μmol m−2 s−1 for KP1 and 1.74 μmol m−2 s−1 for KP2, respectively. Fig. 7 shows the logarithmic plot of the initial flux versus the concentration of KP1 or KP2 for Ag(I) transport. In the case of PIM containing KP1, the flux stabilized at a concentration of 1%, whereas in the case of KP2, the flux changed slightly at a carrier concentration of 3%. Exemplary concentration of carrier, CTA and plasticizer in the membrane are shown in the ESI.† Higher values of metal flux were observed for CTA-based membranes containing 1% KP1 and 3% KP2, while the content of CTA and o-NPPE ranged from 27 to 31% and from 57 to 67%, respectively.
Fig. 8 shows the suggested structure of the complex transported by the liquid phase of the membrane toward the receiving phase where the decomplexing reaction occurs.
Fig. 8 A suggested silver – calixpyrrole (KP1 as well as KP2) complex transported through a plasticized membrane (X− = NO3−). |
The transport of Ag(I) across PIM with KP2 was faster because formation of a complex in membranes took place via both interactions of cations with calixpyrrole i.e. via cavity ring and the carboxylic group. In the case of KP1, additional interaction between the of methylcalixpyrrole group and Ag(I) cation can be neglected and in consequence the formed complex is more labile and the transport of Ag(I) across PIM becomes slower.
The Ag(I) is transported from the source phase to the receiving phase via a plasticized membrane. Movement of the Ag(I) through the PIM is possible due to the presence of the carrier. After complexation of the silver and nitrate ion pair with carrier on the left side of the membrane, the complex diffuses down its concentration gradient. On the right side of the membrane, carrier ion pair complex is decomplexed and silver nitrate ion pair is released into the receiving phase. The free carrier diffuses back across the liquid phase in membrane and the cycle is repeated. The net result is the transport of Ag(I) from the aqueous source phase to the aqueous receiving phase across the organic phase in membrane. A similar transport mechanism is described in the papers31,32 and explained by an increase in the viscosity of organic membrane phase, and thus the resistance of the membrane limiting complex diffusion through the membrane.31
In membrane processes o-nitrophenyl pentyl ether (o-NPPE), was used as the plasticizer of CTA matrix, which had the same concentration of KP1 and KP2 (0.10 M). A series of transport measurements using membrane with a fixed composition of the carrier and matrix (25 mg CTA), plasticizer volume in the range of 0.5–6.0 cm3 per 1.0 g CTA, was performed for the quantitative determination of the optimum content of o-NPPE plasticizer in the membrane (Fig. 9).
Fig. 9 The effect of o-NPPE plasticizer on the Ag(I) transport through PIM. Source phase: 5.0 × 10−4 M AgNO3, pH = 4.0; membrane: 25.0 mg CTA; 0.10 M KP1 and KP2, receiving phase: 0.10 M Na2S2O3. |
Introduction of 4.0 cm3 or more plasticizer solution per 1.0 g CTA did not affect any more the rate of Ag(I) transport through PIM. The membrane thickness for optimum conditions, i.e. 4.0 cm3o-NPPE/1.0 g CTA, was 25 μm. The dissolution of calixpyrroles into the matrix was observed in the case of high content of o-NPPE ether in polymer inclusion membrane, which resulted in the effective transport of Ag(I) ions. Ag(I) ions transport was not observed for the non-plasticized CTA membrane with increasing content of the plasticizer used in the membrane to 4 cm3/1 g CTA in the case of o-NPPE and o-NPOE plasticizers (76% and 77 wt%), the permeability of Ag(I) ions through PIM increased significantly, and then began to stabilize. In the context of these results it should be noted that Raut et al.33 obtained the maximum permeability of cesium(I) ions for CTA membranes containing calix[4]bis-2,3-naphtho-crown-6 and 65% wt o-NPOE. Similar results were presented in the Kaya et al.34 study on the effect of plasticizers for the removal of Cr(IV) using calixarenes in plating bath water. They reported that o-NPPE was the best plasticizer. Using it the best transport efficiency, with recovery of 98%, was achieved. This was expected because o-NPPE has the lowest viscosity and the highest dielectric constant among plasticizer studied.
J i values listed in Table 1 indicate that, compared to PIM with PVC matrix, Ag(I) ions are definitely faster transported through polymer inclusion membranes with CTA matrix. This results from the fact that cellulose triacetate membranes are characterized by stronger hydrophilic properties compared to polyvinyl chloride membranes. This induces the need to provide more ion carriers. Therefore there is a need to increase the share of plasticizer in the membrane with PVC matrix in order to create the inclusion of the organic phase in the membrane of suitable high dispersion degree, i.e. porosity.
CTA-based membranes are more hydrophilic than membranes containing PVC matrix. CTA-based membranes have more expanded and rough surface that allows a better accessibility of the metal ions to the membrane. PVC-based PIMs were more hydrophobic and completely amorphous, and their surface showed less diversity, resulting in worser accessibility.35
Fig. 10 presents the values of recovery factor (RF) as a function of time during a competitive transport of Ag(I) and Cu(II) ions. The selectivity of these membrane systems determined by Ag(I) > Cu(II) order was the highest for PIM containing KP2. After 24 hours, the RF values determined for: KP2 were 98.9% for Ag(I) and 7.2% for Cu(II); KP1 were 80.1% for Ag(I) and 7.1% for Cu(II), respectively. The values of selectivity coefficients are presented in Table 2. They were high due to low affinity of calixpyrroles to Cu(II).
Carrier | Metal ions | Initial flux, Ji [μmol m−2 s−1] | Selectivity coefficient, SM1/M2 |
---|---|---|---|
KP1 | Ag(I) | 0.70 | S Ag(I)/SCu(II) = 10.3 |
Cu(I) | 0.07 | ||
Ag(I) | 0.70 | S Ag(I)/SCd(II) = 15.6 | |
Cd(II) | 0.05 | ||
Ag(I) | 0.70 | S Ag(I)/SZn(II) = 20.0 | |
Zn(II) | 0.04 | ||
KP2 | Ag(I) | 1.60 | S Ag(I)/SCu(II) = 16.0 |
Cu(I) | 0.10 | ||
Ag(I) | 1.60 | S Ag(I)/SCd(II) = 53.3 | |
Cd(II) | 0.03 | ||
Ag(I) | 1.60 | S Ag(I)/SZn(II) = 80.0 | |
Zn(II) | 0.02 |
Studies devoted to the separation ions of Ag(I) and Cd(II) across PIM were also performed. It was found that the transport efficiency of these systems was high for Ag(I) and very low for Cd(II). The separation properties of the membranes relative to the ion Ag(I) and Zn(II) were also checked. After 24 hours, the RF values determined for KP1 and KP2 were 93.66% and 79.45% for Ag(I), respectively. Transport of Cu(II) and Zn(II); Cu(II) and Cd(II), as well as Zn(II) and Cd(II) ions was very slow, and the recovery factor (RF) after 24 hours of the process did not exceed 1%.
Also the selectivity of Ag(I), Cu(II), Cd(II) and Zn(II) ions transport from an equimolar mixture with a concentration of 5.0 × 10−4 M, each through PIM containing KP1 and KP2, was examined in the last stage. The receiving phase was 0.10 M Na2S2O3. Mixtures of metal ions were transported through the membranes for 24 hours, and the values of the fluxes from the competitive transport of Ag(I), Cu(II), Cd(II) and Zn(II) were calculated.
Membrane containing KP2 appeared to be effectively separating Ag(I) ions, other metals were separated much more slowly from the aqueous phase, and their initial fluxes did not exceed the value of 0.10 μmol m−2 s−1. The speed of Ag(I) ions transport by these membrane systems is higher for KP2 in comparison with KP1.
The study on the Ag(I) ions transport in seven measurement cycles (24 hours each) using the same membrane containing 4.0 cm3o-NPPE/1.0 g CTA as well as 0.10 M KP1 and KP2 in the successive cycles, was performed in order to determine the stability of PIM containing calixpyrrole carriers. The selection of PIM composition allowed to obtain SLM membranes of Celgard 2500 type with identical concentrations of KP1 and KP2 as in PIM. Determination of membrane thickness was for PIM and SLM 25 μm.
The values of Ag(I) ions transport fluxes through PIM determined in subsequent measurements were used to estimate the stability of these membranes.
Determined values of the fluxes in successive measurement cycles decreased insignificantly during the transport through PIM containing KP1 and KP2 (Fig. 11). A noticeable decrease in the fluxes of Ag(I) ions transport in case of PIM with KP2 carrier occurred after the fifth measurement cycle, which can be caused by the tendency to form metal salts on the surface of the membrane. Other carriers demonstrated high stability of the transport, and rate changes varied within the range of their standard deviations.9
Similarly, long-term stability measurements were carried out for SLM membranes (Celgard 2500), using the carriers at the same concentration (0.10 M) like in PIM, and o-NPPE solvent – Fig. 12.
The results of long-term transport of Ag(I) ions through SLM (Fig. 12) indicate that the membranes containing the examined calixpyrroles were characterized by a decrease in transport fluxes after 96 hours of the process. All examined membrane systems demonstrated the loss in their stability, which resulted in a rapid reduction in the transport rate after four days of the process.
The possible degradation of surface and the sludge which occurred after the Ag(I) ions transport process (Table 3) were supported by scanning electron microscope (SEM) were analyzed.
The comparison of surface microstructure demonstrates the differentiation in membrane matrix materials in terms of quantity and sediment distribution as a result of the phenomena of Ag(I) ions accumulation in the membrane phase. They are especially evident in the case of SLM membranes with calixpyrroles KP2, as distinct changes in membrane appearance are observed in that case. Crystal structures and sediments which may be metal complexes or carrier were observed in SLM, such only slightly sediments were observed in the PIM membrane, probably caused by in insoluble silver salt formation.
Fig. 13 3D-atomic force microscopy (AFM) images of PIM without carrier (a), PIM containing KP1 (b) as well as PIM containing KP2 (c). |
On all membranes containing KP1 and KP2, well-formed inclusions in the polymer of the matrix containing carrier in the plasticizer solution can be seen. In the case of the polymer inclusion membrane with KP2, the inclusions formed have the shape of elongated drops and the “porosity” is about 50%.
By the use of microscopic methods and in particular atomic force microscopy, it was shown that the membrane of CTA and plasticizer itself is not porous and only slightly corrugated due to the different rate of evaporation of the solvent. On all membranes containing KP1 and KP2 one can see well-formed inclusions in the matrix polymer containing a carrier in plasticizer solution. In the case of the polymer inclusion membrane with KP2, the inclusions of liquid organic phase formed into CTA have the shape of elongated drops and the porosity is about 50%.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra04347k |