DOI:
10.1039/C9RA04638K
(Paper)
RSC Adv., 2019,
9, 26464-26475
Experimental and theoretical research on a new corrosion inhibitor for effective oil and gas acidification
Received
20th June 2019
, Accepted 1st August 2019
First published on 23rd August 2019
Abstract
A new dibenzylamine-quinoline derivative (DEEQ) was synthesized and investigated as a corrosion inhibitor for mild steel in 15% HCl solution in various ways, including via weight loss measurements, contact angle measurements, electrochemical measurements (EIS), scanning electron microscopy (SEM), scanning Kelvin probe (SKP) and theoretical calculations. The experimental results revealed that DEEQ is an effective corrosion inhibitor for oil and gas acidification. In an oil–water two-phase system, the wettability of mild steel can be changed by adsorption, while obeying the Langmuir adsorption isotherm. Finally, quantum chemical calculations and molecular dynamic simulation parameters further show a definite correlation between the theoretical and experimental results.
1. Introduction
Metal acid corrosion not only wastes precious resources and energy but also seriously pollutes the environment. Under the action of corrosion, 10% of the world’s steel output is corroded and consumed each year, especially in the corrosion and rust cleaning of mechanical equipment, pipelines of natural gas and long-distance transmission systems.13 A hydrochloric acid solution not only corrodes equipment, but the acid mist also causes harm to people. Therefore, adding a corrosion inhibitor is an economical and effective method that has received increasing attention.6,7,38
According to the chemical composition, a corrosion inhibitor is divided into two parts: an inorganic portion and an organic inhibitor. The organic inhibitor molecules contain a highly electronegative polar group (O, N, S, etc.), benzene ring, heteroatom ring, double bond or triple bond, and are mostly used in an acidic corrosion medium.4 The unpaired lone pair of electrons or the high electron cloud density region of the bond coordinates with the metal orbital in the form of a coordination bond, and forms a protective film by interface transformation, polymerization and chelation.3,5,35
Most literature reports the use of a Mannich base as a corrosion inhibitor for effective oil and gas acidification.9,36,37,41 Although Mannich bases have a good inhibition effect, there are still many problems that limit their application such as high cost, toxicity and instability. With the enhancement of people’s awareness of environmental protection, research on green corrosion inhibitors represented by quaternary ammonium salt ionic liquids has received more and more attention. At the same time, the hydrophobic chains can align on the metal surface to form a hydrophobic film, which hinders the diffusion of water molecules into the cathode region and inhibits the cathode reaction.17,18 In addition, because of the molecular structure itself, the cations and anions can form a wide range of structures.8,11,12,20 In previous literature, imidazolium-based and benzimidazole ionic liquids were researched as inhibitors for mild steel in acid solution, and the results provide guidance or direction to design and develop new ionic liquids as inhibitors. In particular, the long alkyl chain induced poor water solubility and foaming ability are detrimental for corrosion inhibitors. Thus, short chain and special functional groups became the direction for design. A dibenzylamine-quinoline derivative has not been reported as a corrosion inhibitor, and the properties of good water solubility and stability and the functional groups determine its excellent corrosion inhibition performance. Therefore, in this paper, we synthesized a new corrosion inhibitor, and the mechanism of corrosion between the inhibitor molecule and the mild steel surface was studied. The test methods include weight loss, potentiodynamic polarization, electrochemical impedance spectroscopy (EIS), scanning Kelvin probe (SKP), and scanning electron microscopy (SEM). In addition, the corrosion mechanism was researched further via theoretical quantum chemical calculations and molecular dynamic simulations.
2. Experimental and methods
2.1 Preparation of samples
The composition of the mild steel samples (wt%) was C (0.26%), Si (0.2%), Mn (0.49%), P (0.009%), S (0.004%), Si (0.2%) and Fe for balance. The specimens were tested for weight loss and surface topography analysis was carried out at a size of 50 mm × 10 mm × 3 mm. The mild steel specimen was cleaned ultrasonically with anhydrous ethanol and acetone. After natural drying, the mass of the specimen was accurately weighed using an analytical balance, and the measurement was performed in parallel three times. The results are expressed as average values.
The molecular structure of the inhibitor DEEQ is shown in Fig. 1, and the synthesis was as follows. Dibenzylamine (3.94 g, 20 mmol) was added to a 250 mL single-necked flask with 100 mL ethanol as the solvent. Epichlorohydrin (1.95 g, 21 mmol) was added dropwise, and the reaction was stirred at 50 °C for 16 h. Then rotary evaporation was carried out to remove the solvent and a yellow viscous liquid was obtained. Afterwards, the yellow viscous liquid (2.88 g, 10 mmol) dissolved in 150 mL ethanol was introduced to a 250 mL single-necked flask, and quinoline (1.42 g, 11 mmol) was added to the reaction system, and the system was equipped with a stirrer and a reflux condenser at 80 °C for 12 h. Finally, rotary evaporation was carried out to remove the solvent and after washing with ethyl acetate three times, a white solid was obtained. The 1H NMR measurement was carried out using a Bruker AVANCE III HD 400 NMR Spectrometer. 1H NMR for DEEQ: δ (ppm): 1.1 (1H, m, CH–OH), 1.2 (2H, m, N–CH2), 2.1 (1H, m, CH2–CH–CH2), 3.6–3.8 (4H, m, CH2–N–CH2), 5.2 (2H, m, N+–CH2), 7.2–8.1 (16H, m, Ar-H), 9.0 (1H, m, N+–H).
|
| Fig. 1 Synthetic route to DEEQ. | |
2.2 Contact angle measurements
Contact angles were measured using an automatic tensiometer (GERMAN KRUSS DSA30S) at 20 °C. The experiments were performed under aqueous solution, and the dynamic contact angle was measured by observing the change of contact angle with time in the presence and absence of corrosion inhibitor.
2.3 Weight loss measurements
Weight loss measurements are one of the most reliable methods for determining the uniform corrosion rate and the corrosion inhibitor performance of metals, which is the basis of other test methods.25–27 In the process of the experiment, three samples were suspended from each jar, and the specimens were immersed in a 15% HCl solution with different concentrations of DEEQ for 4 h at 333, 343, 353 and 363 K. The temperature of the solution was kept steady by the water bath, and at the end of the experiment the specimens were removed, the surface washed with water and the corrosion products removed. The specimens were then cleaned with anhydrous ethanol and acetone carefully, and after natural drying the mass of the sample was accurately weighed by an analytical balance, and measured in parallel three times, and the results are expressed as an average value. The corrosion rate was calculated.
2.4 Electrochemical measurements
Electrochemical tests can not only obtain instantaneous data from the metal corrosion process but can also continuously monitor the change in the metal electrode during the corrosion process.2,31 Electrochemical experiments were carried out using the traditional three-electrode system by Reference 3000 (Gamry). A graphite electrode and a saturated calomel electrode (SCE) were used as the auxiliary and reference electrodes, respectively.42,43 In addition, a mild steel electrode was employed as the working electrode with an exposed area of 1.0 cm2. Before starting the experiments, the polished working electrode was cleaned with anhydrous ethanol and acetone and then immersed in the test solution for 20 min to reach a steady potential, and the measurements were performed in the frequency range of 10−2 to 105 Hz with an amplitude of 5 mV at open circuit potential (OCP). The EIS parameters were obtained by fitting the data to an equivalent circuit by using ZSimpWin software. The potentiodynamic polarization curves were obtained in a potential range of −500 mV to 500 mV with a scan rate of 0.5 mV s−1.
2.5 Scanning Kelvin probe
Compared with traditional electrochemical impedance spectroscopy (EIS) technology, scanning Kelvin probe (SKP) technology can analyze the potential distribution on the metal surface, measure the electrochemical properties without contacting the system, and more accurately reflect the characteristics of local corrosion of the metal, which is extremely sensitive to small changes in the interface state. In addition, SKP has high measurement accuracy, and the electrochemical characteristics can be three-dimensionally presented.
The SKP experiment was carried out using a micro area electrochemical scanning system (VersaScan of Princeton Applied Research) at 298 K, using the scan step mode with a scan step size of 100 μm, scan area of 4000 × 4000 μm2, probe vibration amplitude of 30 μm, scan frequency of 80 Hz, and an average distance of the probe from the sample surface of approximately 100 μm. In addition, the SKP system was calibrated with a saturated calomel electrode (SCE) before testing.
2.6 Surface analysis
Surface morphology analysis experiments were carried out using a scanning electron microscope (SEM) (FEI Quanta 450), and the acceleration voltage was 20 kV and the magnification was 150 to 1000 times. SEM can accurately reflect the surface morphology of the metal after corrosion and provides a very valuable reference for the evaluation of corrosion inhibitor performance. Before starting the experiments, the surface should be cleaned with anhydrous ethanol and acetone carefully before natural drying. In this process, the fresh specimen and the specimens immersed in 15% HCl solution in the absence or presence of 6.0 mM DEEQ for 4 h were examined.
2.7 Quantum chemical calculations
The molecular structure parameters of the corrosion inhibitor and the interaction mode and active sites between the molecules and the metal can be obtained through quantum chemical calculations, which provide important information for researching the mechanism of the corrosion inhibitor.19 In the Gaussian 09 program, the geometry of the studied molecules was optimized at the 6-31 g (d, p) basis set level, and the frequency calculation was performed at the same basis level to determine that the found stagnation point was the minimum energy point. After the simulations, the energy of the highest occupied molecular orbital (EHOMO), the energy of the lowest unoccupied molecular orbital (ELUMO), the energy gap (ΔE = ELUMO − EHOMO), the dipole moment (μ), and the Mulliken charge were calculated.
2.8 Molecular dynamic simulations
The Forcite module of Materials Studio was used to model the interaction between inhibitor and iron surface. The calculation model consists of two layers: the surface layer of Fe (100) and the water layer with corrosion inhibitor molecules. The adsorption interface Fe (100) crystal plane thickness is 8 layers, a total of 512 Fe atoms, and the system size is 2.30 nm × 2.30 nm × 1.15 nm. The solvent layer was established using the amorphous Cel I module and consists of an inhibitor molecule and 500 water molecules with a system size of 2.30 nm × 2.30 nm × 2.84 nm. In addition, the temperature was 298.15 K and the integration time step was set to 1 fs. After the simulations the interaction energy (Eint) between the inhibitor molecule and the iron surface was calculated as follows: |
Eint = Etot − Emol − Esur
| (1) |
where Etot is the total energy of the simulation system, Emol is the energy of a free inhibitor molecule, and Esur is the energy of the iron surface together with the water molecules.
3. Results and discussion
3.1 Contact angle measurements
It can be seen from Fig. 2 that the wettability of steel is greatly changed in the presence of DEDB, and because the measurements were performed under aqueous conditions the supplementary angle of the results is the real contact angle. For the fresh steel, the surface contact angle is 78°, which is consistent with the previous reports.1,34 When adding corrosion inhibitor after 1, 2 and 3 hours, the contact angle of the steel is 118°, 127° and 128°, respectively, which indicates that the surface of the steel changed to lipophilic. The DEEQ molecules adsorbed on the steel surface to form the aligned adsorption layer, reducing the free energy of the interface so that water molecules can be displaced more effectively, leading to a high inhibition efficiency.
|
| Fig. 2 The cross sectional optical images of oil droplets on (a) the fresh steel surface, (b) the steel surface inhibited with 7 mM DEEQ after 1 h immersion, (c) the steel surface inhibited with 7 mM DEEQ after 2 h immersion, and (d) the steel surface inhibited with 7 mM DEEQ after 3 h immersion. | |
3.2 Weight loss measurements
The results of the weight loss measurements for mild steel in 15% HCl with different concentrations of DEEQ for 4 h at different temperatures are shown in Table 1. The experimental parameters of corrosion rate (v), inhibition efficiency (η) and surface coverage (θ) were calculated by the following equations:24 |
| (2) |
|
| (3) |
|
| (4) |
where w0 and w are the weight values without and with inhibitor, S is the total surface area of the mild steel specimen, t is the immersion time, θ is the surface coverage, and v0 and v are the corrosion rate of mild steel in the absence and presence of inhibitor, respectively.30
Table 1 Weight loss measurements for mild steel in 15% HCl with different concentrations of DEEQ for 4 h at different temperatures
Temperature (K) |
Concentration (mM) |
v (g m−2 h−1) |
η (%) |
θ |
333 |
Blank |
18.116 |
— |
— |
1.0 |
1.410 |
92.2 |
0.922 |
3.0 |
0.746 |
95.9 |
0.959 |
4.0 |
0.411 |
97.7 |
0.977 |
6.0 |
0.314 |
98.3 |
0.983 |
7.0 |
0.179 |
99.0 |
0.990 |
343 |
Blank |
72.464 |
— |
— |
1.0 |
6.90 |
90.5 |
0.905 |
3.0 |
5.391 |
92.6 |
0.926 |
4.0 |
3.169 |
95.6 |
0.956 |
6.0 |
1.948 |
97.3 |
0.973 |
7.0 |
1.476 |
98.0 |
0.980 |
353 |
Blank |
271.739 |
— |
— |
1.0 |
47.582 |
82.5 |
0.825 |
3.0 |
30.170 |
88.9 |
0.889 |
4.0 |
14.875 |
94.5 |
0.945 |
6.0 |
9.814 |
96.4 |
0.964 |
7.0 |
4.790 |
98.2 |
0.982 |
363 |
Blank |
825.525 |
— |
— |
1.0 |
148.696 |
81.9 |
0.819 |
3.0 |
97.198 |
88.2 |
0.882 |
4.0 |
87.256 |
89.4 |
0.894 |
6.0 |
64.198 |
92.2 |
0.922 |
7.0 |
37.964 |
95.4 |
0.954 |
From Table 1, it was found that with an increase in inhibitor concentration, the corrosion rate decreases, and the inhibitor efficiency and surface coverage increases, which indicates that increasing the concentration leads to an increase in the amount of adsorption. At the same concentration, when the temperature increases the corrosion efficiency decreases. When the concentration of corrosion inhibitor is 7 mmol, the corrosion inhibition rate can reach over 95%, which indicates that DEEQ is an effective inhibitor and can meet the requirements of acidification operation of medium and low temperature oil and gas well.15,24
3.3 Potentiodynamic polarization curves
Fig. 3 shows the potentiodynamic polarization curves for mild steel in 15% HCl solution with and without different concentrations of DHAC at 298 K. The electrochemical parameters of the corrosion potential (Ecorr), corrosion current density (icorr), anodic Tafel slope (βa) and cathodic Tafel slope (βc) obtained by Tafel extrapolation are shown in Table 2, and the calculation formula of the corrosion inhibition efficiency (η) is as follows: |
| (5) |
where icorr and icorr0 are the corrosion densities with and without inhibitor, respectively. From Table 2, it is clear that with the increase in DEEQ concentration, the corrosion current density of the mild steel electrode in the 15% HCl solution decreases, the corrosion efficiency increases, and the corrosion potential shifts negatively. During the linear regions in the anodic and cathodic regions, we can calculate the corrosion parameters, including the corrosion current density, anodic and cathodic Tafel slopes and inhibition efficiency. The corrosion potential on the working electrode in the absence of inhibitor is −0.4071 V. This value shifts towards the cathodic direction in the presence of DEEQ. The values of Ecorr are −0.4382 V, −0.4346 V, −0.43285 V, −0.4284 V and −0.4447 V in the presence of 1 mM, 3 mM, 4 mM, 6 mM and 7 mM, respectively. The values of icorr are 0.6282 mA cm−2, 0.3071 mA cm−2, 0.2450 mA cm−2, 0.1708 mA cm−2, 0.0749 mA cm−2 and 0.0491 mA cm−2 in the absence and presence 1 mM, 3 mM, 4 mM, 6 mM and 7 mM DEEQ, respectively. The reduction of the current densities and the fact that the displacement in Ecorr between the absence and presence of DEEQ is less than 85 mV indicate that DEEQ is a mixed-type inhibitor.8,12
|
| Fig. 3 Polarization curves for mild steel in 15% HCl solution with and without different concentrations of DEEQ at 298 K. | |
Table 2 The electrochemical parameters for mild steel in 15% HCl without and with different concentrations of DEEQ at 298 K
Concentration (mM) |
Ecorr (VSCE) |
icorr (mA cm−2) |
βa (mV dec−1) |
βc (mV dec−1) |
η (%) |
Blank |
−0.4071 |
0.6282 |
62.475 |
−136.7 |
— |
1.0 |
−0.4382 |
0.3071 |
110.0 |
−138.5 |
51.1 |
3.0 |
−0.4346 |
0.2450 |
121.1 |
−123.1 |
61.0 |
4.0 |
−0.4285 |
0.1708 |
110.3 |
−128.7 |
72.8 |
6.0 |
−0.4284 |
0.0749 |
125.4 |
−137.9 |
88.1 |
7.0 |
−0.4447 |
0.0491 |
124.0 |
−144.9 |
92.2 |
From Fig. 3, it was found that the addition of DEEQ had no significant effect on the slope of the cathodic polarization curve of the mild steel electrode in the 15% HCl solution. The approximately parallel cathodic polarization curve indicates that the inhibitor DEEQ has no impact on the mechanism of the reduction of hydrogen, and the process is under activation control.43,44 The addition of DEEQ reduces the number of active sites on the surface of the electrode by adsorption on the mild steel surface, and there was an obvious linear Tafel area on the cathodic polarization curve. It can also be seen from the anodic polarization curve that DEEQ has an evident inhibitory effect on the mild steel electrode at a lower anode potential, which is related to the adsorption of DEEQ on the surface of the mild steel electrode and the formation of a protective layer of inhibitor.10,38 However, when the polarization potential continues to increase, it can be observed that the curves are close to coinciding. This may be due to the rapid dissolution of mild steel at the strong polarization potential, which causes the desorption of DEEQ from the electrode’s surface.
3.4 Electrochemical impedance spectroscopy measurements
Fig. 5 shows the corrosion inhibitory properties of different concentrations of DEEQ in 15% HCl solution at 298 K, as tested using electrochemical impedance spectroscopy (EIS). The equivalent circuit model is displayed in Fig. 4 by fitting the impedance data, which contain the solution resistance (Rs), polarization resistance (Rp) and constant phase element (CPE), and is given in eqn (6):where the CPE is the constant phase element to replace a double layer capacitance Cdl to obtain a more accurate fit of the experimental data set. n corresponds to the phase shift, which is related to the inhomogeneities of the double layer. For n = 0, CPE represents a resistance, for n = 1, a capacitance and for n = −1 an inductance. The dimension of Y0 is sn Ω−1, while that of a capacitance (C) is s Ω−1 or F. Despite this difference, Y0 is often used as if it were the capacitance of the corroding system. Conversion of Y0 data into C is very important when experimental capacitance data are to be used to determine quantitatively system parameters.14,40 The “double layer capacitance” values (Cdl) are calculated as follows: |
| (7) |
where is the angular frequency corresponding to the maximum imaginary part of the impedance spectrum. The impedance parameters are displayed in Table 3 and the inhibition efficiency (η) was calculated by the following equation: |
| (8) |
where Rp and R0p are the polarization resistance (Ω cm2) with and without DEEQ, respectively. From Fig. 4(a), it is clear that the Nyquist figure displays a depressed capacitive loop, and with the increase in DEEQ concentration, the radius of the capacitive loop increases, which means that the charge transfer between the solution and mild steel is dramatically hindered by the addition of DEEQ.21,24 In addition, the fact that there is no change in the shape of the impedance spectra with the addition of inhibitor indicates that the presence of the inhibitor has no influence on the corrosion mechanism. The Bode and phase angle plots for mild steel in the 15% HCl solution with different concentrations of DEEQ are displayed in Fig. 4(b). The phase angles of the blank and inhibited solutions are 66° at 197 Hz, 69° at 157 Hz, 70° at 60 Hz, 71° at 54 Hz, 72° at 200 Hz and 74° at 199 Hz, and with the increase in inhibitor concentration, the absolute impedance gradually increases at low frequencies, which indicates that DEEQ has the higher inhibitory effect.28 It can be found from Table 3 that with the increase in the DEEQ concentration, R0p increases, which indicates that the inhibitor has an evident inhibitory effect after adsorption on the mild steel surface. The minimum polarization resistance (Rp) of the blank solution is 109.4 Ω cm2, the maximum value of R0p reaches 1313 Ω cm2 when the concentration is 7.0 mM, and η is 91.2%. In addition, with the increase in inhibitor concentration the value of the electric double layer capacitance decreases, which is attributed to the inhibitor molecules replacing the water molecules adsorbed on the mild steel surface.
|
| Fig. 4 EIS for mild steel in a 15% HCl solution with and without different concentrations of DEEQ at 298 K: (a) Nyquist plots and (b) Bode plots. | |
|
| Fig. 5 Equivalent circuit used to fit the obtained impedance spectra for mild steel in a 15% HCl solution. | |
Table 3 The EIS parameters for mild steel in 15% HCl solution without and with different concentrations of DEEQ at 298 K
C (mM) |
Rs (Ω cm2) |
Rp (Ω cm2) |
Y0 × 104 (Ω−1 sn cm−2) |
n |
Cdl (μF cm−2) |
η (%) |
0 |
1.76 |
109.4 |
2.17 |
0.89 |
114.6 |
— |
1.0 |
1.31 |
596.9 |
1.85 |
0.80 |
84.6 |
81.2 |
3.0 |
1.50 |
731.6 |
1.20 |
0.83 |
66.8 |
85.0 |
4.0 |
1.30 |
772.1 |
1.04 |
0.81 |
49.1 |
85.8 |
6.0 |
1.38 |
1037 |
0.90 |
0.81 |
41.9 |
89.4 |
7.0 |
1.25 |
1313 |
0.69 |
0.85 |
38.9 |
91.2 |
3.5 Scanning Kelvin probe
Fig. 6 shows the three-dimensional diagram of potential distribution for the original state (a), and the absence (b) and presence (c) of DEEQ in 15% HCl for 4 h at 298 K. It is clear that the potential distribution of the original state has a negative potential value, and the uneven potential distribution was mainly due to differences in roughness of the specimen surface. Comparing the original state with the result in the absence of DEEQ, the potential distribution of the specimen surface is distinctly positive, which indicates that the surface of the specimen was corroded, causing the potential to move in the positive direction. For the result in the presence of DEEQ (c), the potential distribution was again a negative value, which means that the specimen’s surface was effectively protected with the inhibitor, and proves that DEEQ has excellent performance as an inhibitor, corresponding with the inhibitor performance obtained from the weight loss and electrochemical experiments.
|
| Fig. 6 Three-dimensional diagrams of the potential distributions for the original state (a), and the absence (b) and presence (c) of DEEQ in 15% HCl for 4 h at 298 K. | |
Fig. 7 is the GaussAmp fitting curve of the SKP potential distribution on the surface of the specimens in the original state, and in the absence and presence of DEEQ in 15% HCl for 4 h at 298 K, and the fitting formula is shown in the follow equation:
|
| (9) |
where
A is constant,
y0 is the ordinate offset,
xc is the concentrated position of the potential distribution,
w2 is the degree of concentration, and the smaller the value, the more concentrated the potential distribution at the
xc value. From the fitting results we find the
xc values of the original state, and in the absence and presence the DEEQ are −803 (mV), 98 (mV) and −213 (mV), respectively.
|
| Fig. 7 Histogram of potential distributions and fitting curves of the original state (A), and in the absence (B) and presence (C) of DEEQ. | |
3.6 Adsorption isotherm studies and thermodynamic analysis
Many literature reports have indicated that organic corrosion inhibitors mainly achieve their inhibitory effects through adsorption on mild steel surfaces, so adsorption isotherm studies can provide more information regarding the interaction between the inhibitor and the mild steel surface. In this part, the classical Langmuir adsorption isotherm was applied to describe the adsorption behavior of DEEQ, and the isotherm can be represented as: |
| (10) |
where Kads is the equilibrium constant of the adsorption process, C is the concentration of inhibitor and θ is the surface coverage. All of the parameters can be obtained from the weight loss measurement. In addition, the thermodynamic parameters of standard free energy (ΔG0ads), enthalpy (ΔH0ads) and entropy (ΔS0ads) are calculated by the following equations: |
| (11) |
|
| (12) |
where R is the universal gas constant, T is the thermodynamic temperature, and the value of 55.5 is the molar concentration of water in the solution (mol L−1). From Fig. 8 it is clear that there is an obvious linear relationship between C/θ and C, and the value of the regression coefficient (R) is close to 1 at different temperatures, which indicates that the adsorption of DEEQ on the mild steel surface obeys the Langmuir adsorption isotherm.23,26,29 Table 4 shows the parameters of adsorption thermodynamics, and it can be found that there is a negative value of ΔG0ads at different temperatures, indicating that the adsorption of DEEQ on the surface of mild steel is a spontaneous process. Furthermore, the values of ΔG0ads are concentrated around −33 kJ mol−1, which indicates that the adsorption of DEEQ on the surface of mild steel is a mixed adsorption, and the results correspond with the data obtained from the electrochemical experiments. In addition, a negative ΔH0ads reveals that the adsorption of DEEQ on the metal surface in 15% HCl is a exothermic process (Fig. 9).32,33
|
| Fig. 8 Langmuir adsorption plots for mild steel in 15% HCl solution with different concentrations of DEEQ at different temperatures. | |
Table 4 Thermodynamic parameters of adsorption for mild steel in 15% HCl solution at different temperatures
T (K) |
Kads (L mol−1) |
ΔG0ads (kJ mol−1) |
ΔH0ads (kJ mol−1) |
ΔS0ads (J K−1 mol−1) |
333 |
9336 |
−36.41 |
−39.77 |
−77.1 |
343 |
6234 |
−36.35 |
353 |
3222 |
−35.48 |
363 |
3128 |
−36.39 |
|
| Fig. 9 The relationship between lnKads and (1000/T) for mild steel in 15% HCl solution with different concentrations of DEEQ. | |
3.7 Surface analysis
Fig. 10 shows the SEM micrographs of the fresh specimen (a) and the specimens after immersion in 15% HCl solution in the presence (b) and absence (c) of 7.0 mM DEEQ for 4 h at 363 K. It can be seen from the images that the surface of the specimen is seriously damaged in the absence of inhibitor due to the corrosive acid solution,22,23 and the specimen shows a smooth surface in the presence of inhibitor. In addition, elemental analysis was carried out by using energy dispersive spectroscopy (EDS), and the results are shown in Table 5. Comparing the samples in the absence and presence inhibitor, the content of the element N increased significantly, indicating that an adsorption film was formed on the surface of the specimen,16–18 which isolated the acid solution and protected the specimen. These results are consistent with the inhibitor performance results obtained from the weight loss, SKP, adsorption isotherm and electrochemical experiments.
|
| Fig. 10 SEM micrographs of the mild steel surface before (a) and after immersion in 15% HCl solution with (b) and without (c) DEEQ for 4 h at 298 K. | |
Table 5 Element analysis of the mild steel surface before and after immersion in 15% HCl solution without DEEQ for 4 h at 298 K
Element |
C |
N |
O |
Si |
Mn |
Fe |
Before |
wt% |
00.15 |
— |
03.99 |
00.67 |
01.72 |
93.47 |
at% |
00.63 |
— |
12.53 |
01.20 |
01.57 |
84.06 |
After |
wt% |
0.11 |
2.41 |
7.39 |
0.61 |
1.87 |
87.60 |
at% |
0.42 |
7.59 |
20.38 |
0.96 |
1.50 |
69.15 |
3.8 Quantum chemical calculations
In order to further understand the corrosion inhibition mechanism of DEEQ, quantum chemical calculations were performed. The optimized geometry structure of DHAC and the electron density distributions of the HOMO and LUMO are displayed in Fig. 11 and Table 6 shows the associated quantization parameters such as EHOMO, ELUMO, ΔE and the dipole moment μ. It can be seen that the electron density distributions of both the HOMO and LUMO are evenly distributed on the benzene ring, indicating the benzene ring is the active site of adsorption.39 On the other hand, because of the plane conjugated structure, the inhibitor DEEQ is considered to adsorbed smoothly on the surface of the mild steel.
|
| Fig. 11 Optimized geometric structure (a) and the electron density distributions of the HOMO (b) and LUMO (c) for the DEEQ cation. | |
Table 6 Quantum chemical parameters for the DEEQ cation
HOMO (eV) |
LUMO (eV) |
ΔE (eV) |
μ (D) |
−8.43009172 |
−6.052359588 |
2.377732132 |
10.748355 |
According to frontier molecular orbital theory, the reactivity of the molecule is closely related to the highest occupied molecular orbital (HOMO) and the lowest unoccupied molecular orbital (LUMO).18 The HOMO and LUMO orbits are related to the ability of the molecule to give and accept electrons, respectively. A high EHOMO value means that the molecule has a strong electron donating ability, and the lower the ELUMO value the easier the molecule accepts electrons. Therefore, when the corrosion inhibitor molecules have a high EHOMO and low ELUMO, the electron transfer between the inhibitor molecules and the metal surface is easy, and the inhibitor shows high corrosion inhibition performance.45 From Table 6, both the EHOMO and ELUMO values are lower, which means that the DEEQ cation accepts electrons more easily than it donates electrons. Compared with the tiny μ value of H2O, the DEEQ cation is more likely to replace the water molecules adsorbed on the surface of mild steel.
Table 7 shows the Mulliken charges of the atoms in the DEEQ cation. It was found that the charges of C2, C9, C11, C22, C24 and C26 are positive, while the charges of the benzene ring are negative, and the net charge of all the atoms of DEEQ is negative. Therefore, the conjugated benzene ring can offer electrons to form a coordinate bond with the metal orbital. In addition, the site of the positive charge can accept electrons to interact with the metal surface by electrostatic attraction, which all indicates that DEEQ can easily adsorb on the metal’s surface.
Table 7 The Mulliken charge of atoms in the DEEQ cation
Atom |
N1 |
N2 |
O1 |
C2 |
C3 |
C4 |
C5 |
C6 |
C7 |
Mulliken charge |
−0.4845 |
−0.3892 |
−0.6470 |
0.1391 |
−0.1806 |
−0.1271 |
−0.1345 |
−0.2145 |
−0.1296 |
C8 |
C9 |
C10 |
C11 |
C12 |
C13 |
C14 |
C15 |
C16 |
C17 |
−0.1634 |
0.1091 |
−0.2291 |
0.3403 |
−0.1871 |
−0.1273 |
−0.1275 |
−0.1304 |
−0.1132 |
−0.2030 |
C18 |
C19 |
C20 |
C21 |
C22 |
C23 |
C24 |
C25 |
C26 |
C27 |
−0.1297 |
−0.1650 |
−0.1567 |
−0.2037 |
0.1272 |
−0.1836 |
0.1337 |
−0.2036 |
0.1190 |
−0.0982 |
3.9 Molecular dynamic simulations
In order to research the microscopic behavior of the inhibitor adsorbed on the mild steel Fe (100) surface, the equilibrium configuration for DEEQ in an aqueous system was simulated, and the result is shown in Fig. 12. It can be seen that the DEEQ cation is parallel with the Fe (100) surface, which indicates that the planar structure of the dibenzylamine ring is the dominant factor for the adsorption orientation. In an aqueous system, the DEEQ molecules have a strong mutual attraction between the active sites and the Fe (100) surface, causing the inhibitor molecules to be immobilized on the metal surface. The kinetic simulation results show that the adsorption energy of the molecule is −2174.93 kJ mol−1, which is much larger than that of the water molecules on the Fe (100) surface of −24.64 kJ mol−1,24 indicating that the inhibitor molecules can expel the water molecules and adsorbed on the Fe (100) surface. It can be inferred that the inhibitor molecules can aggregate and adsorb on the metal surface to form a dense molecular film layer in the liquid phase corrosive medium, separating the metal surface from the water molecules and the corrosive medium to achieve the effect of corrosion inhibition.
|
| Fig. 12 Equilibrium configuration of DEEQ in an aqueous system (side view and top view). | |
4. Conclusion
Weight loss and SEM measurements revealed that DEEQ is an effective inhibitor through adsorption on the mild steel surface, blocking contact between the acidic medium and metal surface, and the inhibitor exhibited a 95.4% maximum inhibition efficiency at 363 K, which can meet the requirements of acidification operation of medium and low temperature oil and gas well. The contact angle experiment shows that the corrosion inhibitor can change the wettability of the steel sheet surface, thus inhibiting acid corrosion of oil and gas string. Electrochemical experiments showed that DEEQ can inhibit both the anodic and cathodic corrosion processes, and indicated that DEEQ is a mixed inhibitor. From the microscopic point of view, scanning Kelvin probe (SKP) experiments further proved that DEEQ has an obvious inhibitory effect, and the adsorption of DEEQ on mild steel obeys the Langmuir adsorption isotherm. Theoretical calculations revealed that the DEEQ molecules can provide electrons to the metal atomic orbital with a strong interaction. The results further demonstrated that DEEQ has an evident inhibitory effect for oil and gas field acidification.
Conflicts of interest
There are no conflicts to declare.
Acknowledgements
This work was supported by the Sichuan Youth Science and Technology Innovation Research Team Program (2017TD0013) and the Major Program of the National Natural Science Foundation of China (Grant No. 51490653).
References
- A. Alagta, I. Felhösi and I. Bertoti, et al., Corrosion protection properties of hydroxamic acid self-assembled monolayer on carbon steel, Corros. Sci., 2008, 50(6), 0–1649 CrossRef CAS.
- M. T. Alhaffar, S. A. Umoren and I. B. Obot, et al., Isoxazolidine derivatives as corrosion inhibitors for low carbon steel in HCl solution: experimental, theoretical and effect of KI studies, RSC Adv., 2018, 8(4), 1764–1777 RSC.
- J. Aljourani, K. Raeissi and M. A. Golozar, Benzimidazole and its derivatives as corrosion inhibitors for mild steel in 1 M HCl solution, Corros. Sci., 2009, 51(8), 0–1843 CrossRef CAS.
- P. Arellanes-Lozada, O. Olivares-Xometl and N. V. Likhanova, et al., Adsorption and performance of ammonium-based ionic liquids as corrosion inhibitors of steel, J. Mol. Liq., 2018, 151–163 CrossRef CAS.
- F. Bentiss, C. Jama and B. Mernari, et al., Corrosion control of mild steel using 3,5-bis(4-methoxyphenyl)-4-amino-1,2,4-triazole in normal hydrochloric acid medium, Corros. Sci., 2009, 51(8), 0–1635 CrossRef.
- D. Daoud, T. Douadi and H. Hamani, et al., Corrosion inhibition of mild steel by two new S-heterocyclic compounds in 1 M HCl: Experimental and computational study, Corros. Sci., 2015, 94, 21–37 CrossRef CAS.
- Q. Deng, N. N. Ding, X. L. Wei, L. Cai, X. P. He and Y. T. Long, Identification of diverse 1,2,3-triazole-connected benzyl glycoside-serine/threonine conjugates as potent corrosion inhibitors for mild steel in HCl, Corros. Sci., 2012, 64(6), 64–73 CrossRef CAS.
- A. A. Farag, A. S. Ismail and M. A. Migahed, Environmental-friendly shrimp waste protein corrosion inhibitor for carbon steel in 1 M HCl solution, Egypt. J. Pet., 2018, 1187–1194 CrossRef.
- H. X. Feng, J. Li and X. H. Gao, Electrochemical Studies of some New Mannich Bases Compounds as Corrosion Inhibitors for Mild Steel in Acidic Media, Adv. Mater. Res., 2012, 538–541, 2329–2333 CAS.
- A. S. Fouda, M. A. Ismail and A. S. Abousalem, et al., Experimental and theoretical studies on corrosion inhibition of 4-amidinophenyl-2,2′-bifuran and its analogues in acidic media, RSC Adv., 2017, 7(73), 46414–46430 RSC.
- H. J. Habeeb, H. M. Luaibi and R. M. Dakhil, et al., Development of new corrosion inhibitor tested on mild steel supported by electrochemical study, Results Phys., 2018, 1260–1267 CrossRef.
- H. Hamani, T. Douadi and D. Daoud, et al., 1-(4-Nitrophenylo-imino)-1-(phenylhydrazono)-propan-2-one as corrosion inhibitor for mild steel in 1 M HCl solution: Weight loss, electrochemical, thermodynamic and quantum chemical studies, J. Electroanal. Chem., 2017, 801, 425–438 CrossRef CAS.
- K. Haruna, I. B. Obot and N. K. Ankah, et al., Gelatin: A green corrosion inhibitor for carbon steel in oil well acidizing environment, J. Mol. Liq., 2018, 264, 515–525 CrossRef CAS.
- F. Mansfeld and C. H. Hsu, Concerning the conversion of the constant phase element parameter y0 into a capacitance, Corrosion, 2001, 57, 747–748 CrossRef.
- Z. Hu, Y. Meng and X. Ma, et al., Experimental and theoretical studies of benzothiazole derivatives as corrosion inhibitors for carbon steel in 1 M HCl, Corros. Sci., 2016, 112, 563–575 CrossRef CAS.
- E. B. Ituen, O. Akaranta and S. A. Umoren, N-Acetyl cysteine based corrosion inhibitor formulations for steel protection in 15% HCl solution, J. Mol. Liq., 2017, 112–118 CrossRef CAS.
- S. John and A. Joseph, Electro analytical, surface morphological and theoretical studies on the corrosion inhibition behavior of different 1,2,4-triazole precursors on mild steel in 1 M hydrochloric acid, Mater. Chem. Phys., 2012, 133(2–3), 1083–1091 CrossRef CAS.
- O. Kaczerewska, R. Leiva-Garcia and R. Akid, et al., Efficiency of cationic Gemini surfactants with 3-azamethylpentamethylene spacer as corrosion inhibitors for stainless steel in hydrochloric acid, J. Mol. Liq., 2017, 247, 6–13 CrossRef CAS.
- L. Guo, S. Zhu and S. Zhang, et al., Theoretical studies of three triazole derivatives as corrosion inhibitors for mild steel in acidic medium, Corros. Sci., 2014, 87, 366–375 CrossRef CAS.
- S. Masroor, M. Mobin and M. J. Alam, et al., The novel iminium surfactant p-benzylidene benzyldodecyl iminium chloride as a corrosion inhibitor for plain carbon steel in 1 M HCl: electrochemical and DFT evaluation, RSC Adv., 2017, 7(37), 23182–23196 RSC.
- P. Mayakrishnan, S. H. Kim and H. Venkatesan, et al., Rhus verniciflua as a green corrosion inhibitor for mild steel in 1 M H2SO4, RSC Adv., 2016, 6(62), 2046–2069 Search PubMed.
- N. A. Negm, A. M. A. Sabagh and M. A. Migahed, et al., Effectiveness of some diquaternary ammonium surfactants as corrosion inhibitors for carbon steel in 0.5 M HCl solution, Corros. Sci., 2010, 52(6), 0–2132 CrossRef.
- A. Popova, M. Christov and A. Vasilev, et al., Mono- and dicationic benzothiazolic quaternary ammonium bromides as mild steel corrosion inhibitors. Part I: Gravimetric and voltammetric results, Corros. Sci., 2011, 53(2), 0–686 CrossRef.
- Q. Ma, S. Qi and X. He, et al., 1,2,3-Triazole derivatives as corrosion inhibitors for mild steel in acidic medium: Experimental and computational chemistry studies, Corros. Sci., 2017, 129, 91–101 CrossRef CAS.
- Y. Qiang, S. Zhang and B. Tan, et al., Evaluation of Ginkgo leaf extract as an eco-friendly corrosion inhibitor of X70 steel in HCl solution, Corros. Sci., 2018, 6–16 CrossRef CAS.
- Z. Salarvand, M. Amirnasr and M. Talebian, et al., Enhanced corrosion resistance of mild steel in 1 M HCl solution by trace amount of 2-phenyl-benzothiazole derivatives: Experimental, quantum chemical calculations and molecular dynamics (MD) simulation studies, Corros. Sci., 2017, 114, 133–145 CrossRef CAS.
- T. A. Salman, K. F. Al-Azawi and M. I. Mahdi, et al., Experimental studies on inhibition of mild steel corrosion by novel synthesized inhibitor complemented with quantum chemical calculations, Results Phys., 2018, 10, 291–296 CrossRef.
- S. M. Shaban, N-(3-(Dimethyl benzyl ammonio) propyl) alkanamide chloride derivatives as corrosion inhibitors for mild steel in 1 M HCl solution: experimental and theoretical investigation, RSC Adv., 2016, 6(46), 39784–39800 RSC.
- A. K. Singh and M. A. Quraishi, The effect of some bis-thiadiazole derivatives on the corrosion of mild steel in hydrochloric acid, Corros. Sci., 2010, 52(4), 0–1385 Search PubMed.
- A. K. Singh and M. A. Quraishi, Investigation of the effect of disulfiram on corrosion of mild steel in hydrochloric acid solution, Corros. Sci., 2011, 53(4), 0–1297 CrossRef.
- V. V. Torres, R. S. Amado and C. Faia de Sá, et al., Inhibitory action of aqueous coffee ground extracts on the corrosion of carbon steel in HCl solution, Corros. Sci., 2011, 53(7), 0–2392 CrossRef CAS.
- X. Wang, H. Yang and F. Wang, An investigation of benzimidazole derivative as corrosion inhibitor for mild steel in different concentration HCl solutions, Corros. Sci., 2011, 53(1), 0–121 Search PubMed.
- X. Wang, H. Yang and F. Wang, A cationic Gemini-surfactant as effective inhibitor for mild steel in HCl solutions, Corros. Sci., 2010, 52(4), 0–1276 Search PubMed.
- W. Wu, M. Chen and S. Liang, et al., Superhydrophobic surface from Cu–Zn alloy by one step O2 concentration dependent etching, J. Colloid Interface Sci., 2008, 326(2), 478–482 CrossRef CAS PubMed.
- K. Xhanari, M. Finšgar and M. Knez Hrnčič, et al., Green corrosion inhibitors for aluminium and its alloys: a review, RSC Adv., 2017, 7(44), 27299–27330 RSC.
- Y. Xiu-Fang, T. Min-Min and M. A. Yang-Min, Mannich Base as Corrosion Inhibitor for N80 Steel in HCl Solution, Surf. Technol., 2017, 175–181 Search PubMed.
- J.-Q. Xue, X.-N. Ma, L.-H. Yu, C.-B. Tang and J. Ma, Development of a novel acidification corrosion inhibitor for P110 steel at high temperature, Sci. Adv. Mater., 2012, 4(1), 61–67 CrossRef CAS.
- X. Yang, F. Li and W. Zhang, 4-(Pyridin-4-yl) thiazol-2-amine as an efficient non-toxic inhibitor for mild steel in hydrochloric acid solutions, RSC Adv., 2019, 9(19), 10454–10464 RSC.
- N. Yilmaz, A. Fitoz and ÿ. Ergun, et al., A Combined Electrochemical and Theoretical
Study into the Effect of 2-((thiazole-2-ylimino) methyl) phenol as a Corrosion Inhibitor for Mild Steel in a Highly Acidic Environment, Corros. Sci., 2016, 110–120 CrossRef CAS.
- R. Yıldız, An electrochemical and theoretical evaluation of 4,6-diamino-2-pyrimidinethiol as a corrosion inhibitor for mild steel in HCl solutions, Corros. Sci., 2014, 90, 544–553 CrossRef.
- Y. Pan, F. Zhan, Z. Lu and Y. Lin, A Mannich base 1-phenyl-3-(1-pyrrolidinyl)-1-propanone: synthesis and performance study on corrosion inhibition for N80 steel in 15% hydrochloric acid, Anti-Corros. Methods Mater., 2016, 63(2), 153–159 CrossRef.
- D. Zhang, Y. Tang and S. Qi, et al., The inhibition performance of long-chain alkyl-substituted benzimidazole derivatives for corrosion of mild steel in HCl, Corros. Sci., 2015, 102, 517–522 CrossRef.
- X. Zheng, S. Zhang, W. Li, L. Yin, J. He and J. Wu, Investigation of 1-butyl-3-methyl-1H-benzimidazolium iodide as inhibitor for mild steel in sulfuric acid solution, Corros. Sci., 2014, 80(3), 383–392 CrossRef CAS.
- X. Zheng, S. Zhang, W. Li, M. Gong and L. Yin, Experimental and theoretical studies of two imidazolium-based ionic liquids as inhibitors for mild steel in sulfuric acid solution, Corros. Sci., 2015, 95, 168–179 CrossRef CAS.
- L. Zhou, Y. L. Lv and Y. X. Hu, et al., Experimental and theoretical investigations of 1,3,5-tris(4-aminophenoxy) benzene as an effective corrosion inhibitor for mild steel in 1, M HCl, J. Mol. Liq., 2018, 249, 179–187 CrossRef CAS.
|
This journal is © The Royal Society of Chemistry 2019 |
Click here to see how this site uses Cookies. View our privacy policy here.