High intrinsic activity of the oxygen evolution reaction in low-cost NiO nanowall electrocatalysts

Salvatore Cosentino *a, Mario Urso *ab, Giacomo Torrisi b, Sergio Battiato b, Francesco Priolo b, Antonio Terrasi b and Salvo Mirabella ab
aIMM-CNR and Università di Catania, via S. Sofia 64, 95123, Catania, Italy. E-mail: salvo.cosentino@gmail.com
bDipartimento di Fisica e Astronomia “Ettore Majorana”, Università di Catania, via S. Sofia 64, 95123, Catania, Italy. E-mail: mario.urso@dfa.unict.it

Received 1st July 2020 , Accepted 28th July 2020

First published on 28th July 2020


Abstract

Earth-abundant materials for electrochemical water splitting typically show a lower efficiency than noble and rare metal electrocatalysts. Nanostructuring and appropriate material design can largely improve the performances of low-cost electrocatalysts, opening the route towards profitable mass production. Here, we report on a quantitative investigation of the oxygen evolution reaction (OER) on Ni-based nanowall (NW) electrodes. The NiO and Ni(OH)2 NW films (200 or 400 nm thick) are produced by chemical bath deposition followed by calcination at 350 °C. The morphology and the chemical arrangement of the NW were studied, before and after the OER, by scanning electron microscopy, energy dispersive X-ray analysis and X-ray photoelectron spectroscopy. The OER electrocatalytic activity was investigated by electrochemical measurements under alkaline conditions (1 M KOH), demonstrating a stable overpotential of 345 mV at 10 mA cm−2, a Tafel slope of 48 mV dec−1 and an O2 turnover conversion frequency (TOF) of up to 0.18 s−1. The quantitative measurement of active electrocatalysts, through cross-correlation of the experimental data, shows nearly 100% material utilization in the 200 nm NiO NW. In thicker NiO or Ni(OH)2 NW films this fraction decreases below 60%, probably due to the decrease in the electric potential along the nanostructure, as revealed by numerical simulation. These data and discussion support the use of low-cost Ni-based nanostructures for high-efficiency and sustainable electrocatalysts.


Introduction

Electrochemical water splitting represents a pivotal technology to produce energy in a sustainable, clean and diffuse way.1–4 The process of water splitting typically proceeds through two half reactions occurring at two electrodes: the cathodic hydrogen evolution reaction (HER) and the anodic oxygen evolution reaction (OER), which in the case of alkaline media can be summarized as:1,2
4H2O + 4e → 2H2 + 4OH and 4OH → O2 + 2H2O + 4e
The main intrinsic limitation of this technology is related to the poor efficiency of the OER process, associated with slow reaction kinetics and high values of overpotential required for the formation of O2 through several intermediate reactions.1,5,6 The low efficiency of the OER is potentially detrimental also for the HER process and the final H2 conversion, since the two half-reactions proceed together in a complete electrochemical water splitting device. To date, Ir- and Ru-oxides have been the best reference electrocatalysts known for the OER, while Pt-coated electrodes have been used to efficiently drive the HER.1,4,7 However, the cost and low abundance of these electrocatalysts pose questions regarding their large-scale usage and thus numerous efforts have been directed towards the development of effective catalysts by using nanostructured and Earth abundant materials.4 Among the plethora of materials and compounds recently proposed as low-cost OER electrocatalysts,7–10 transition metal oxides and oxy-hydroxide nanomaterials are unquestionably promising candidates in large-scale electrochemical water splitting.11–13 In particular, Ni-oxide nanomaterials are well-assessed Earth abundant materials for efficient OER, especially in combination with other metal dopants.4,5,11,14–16 NiO-based nanostructures have already shown very proficient catalytic actions in sensing, electrochromical smart windows, supercapacitors and energy applications.17–23 Such materials have great potential to work also as an efficient backbone-platform electrocatalyst for both the HER and the OER. Doping or alloying with Fe, Co, and Mn shows a large improvement in the performance of the Ni electrocatalyst for the OER, probably due to the optimization of the OH bonding within the active sites.11,14 On the other side, alloying Ni with P or Mo shows a beneficial effect also for the HER.24–27 Ni-based nanostructures are thus extremely appealing as a full water splitting cell can be realized with bi-functional heterogeneous electrocatalytic sites for the HER and the OER.16 It has been recently shown that Ni–Co–Fe sulphide nanosheets on Ni nanocones act as high performance electrocatalysts for total electrochemical water splitting at a potential of 1.54 V to give a current density of 10 mA cm−2.28 Similarly, Fe2+-doped layered double (Ni, Fe) hydroxides are used for overall water splitting showing an overpotential of 1.54 V to give a current density of 10 mA cm−2.29 In photoelectrochemical water splitting the superior performance of Ni nanostructures in comparison to that of Ni dense materials has largely been shown and attributed to a more effective charge transfer process.30,31

Actually, there is currently great efforts within the materials science community to find electrocatalysts with superior performance for water splitting, and the nanotechnology approach greatly supports the progress in this direction.4,5,16 Nonetheless, while many papers report encouraging enhancements of the catalytic action when Ni(oxide) nanostructures are mixed with other elements, a net discrimination of the doping effect over the nanostructure advantages and a fundamental understanding of both are sometimes missing. In addition, a high loading of material electrocatalysts, as typically occurs for Earth abundant elctrocatalysts, could be as expensive as for noble-metal electrocatalysts due to their lower intrinsic activity.4 This highlights that for a real large-scale usage of water splitting methods, a clear determination of the mass activity is needed. Moreover, a fair comparison among the literature data and the reproducible results is still quite a challenge. It was magisterially shown that just a few nanomolar levels of Ni and Fe impurities in the electrolyte solution, coming from contaminated chemicals or glassware, are able to give rise to an OER current of up to 1 mA at an overpotential of 400 mV.32,33 Therefore, controlled and reproducible experiments with quantitative metrics, and hopefully a solid understanding of the underlying mechanism, are urgently needed when a new performant electrocatalyst is claimed.1 Besides the ability to drive the efficient synthesis of nanostructures and to obtain the best usage of material resources, it would be as desirable to reliably measure the quantitative utilization of the catalytic material, which could help in developing specific shape, size and alloying of elements and compounds for efficient OER.

Here we report on a detailed and quantitative investigation of the OER in low-cost synthesized Ni-oxide based nanowalls (NW) without any intentional doping. Ni(OH)2 and NiO NW are carefully synthesized by chemical bath deposition and both show a highly textured surface leading to effective ion exchange with the electrolyte. Electrochemical measurements show improved stability and high OER conversion efficiency in the thin NiO NW, while significant unused materials are estimated for the thick NW films. Numerical modelling of the electrical potential distribution along the NW explains the more effective electrochemical activation of the shorter NW, which is further corroborated by quantitative XPS analysis. These data and relative discussion shed a new light on the basic mechanisms of the OER process in Ni-based nanostructures.

Experimental

Particular care was taken to avoid any potential Fe contamination sources during all the experimental processes. The Ni(OH)2 NW was grown on cleaned substrates by chemical bath deposition (CBD) using new and Fe-free Teflon beakers. The substrates consisted of thin films of Au (50 nm) on Ti (25 nm) grown on quartz substrates by sputtering deposition. Quartz substrates were chosen on purpose to avoid Fe contamination and were carefully cleaned with acetone, isopropanol and DI water and dried in N2 before deposition. The chemical solution for CBD was prepared by mixing 0.42 M NiSO4·6H2O (Alfa Aesar, 98%), 0.07 M K2S2O8 (Alfa Aesar, 97%) and 3.5 wt% ammonia (Merck, 30–33 wt% NH3 in H2O) in DI water.22 The solution was heated up to 50 °C and kept at this temperature using a bain-marie setup. The substrates were immersed in CBD solution for a period of time ranging from 3 to 20 min, in order to achieve growth of Ni(OH)2 NW films with different thicknesses. Then, the samples were rinsed with deionized water to wash the deposited film from the unwanted microparticulate and dried in N2. Some samples were further annealed at 350 °C for 60 min in Ar in order to achieve calcination of films and obtain the NiO NW, as confirmed by XRD.17 The film mass after each synthesis step was measured with a Kern ABT-100 5NM (sensitivity of 0.01 mg) quartz micro-balance (QCM).

The surface morphology and the sample thickness were characterized by using a scanning electron microscope (Gemini field emission SEM Carl Zeiss SUPRA 25) combined with energy dispersive X-ray spectroscopy (EDX).

Electrochemical analyses were performed using a Versastat-4 potentiostat in a three-electrode setup with Pt wire as the cathode, a saturated calomel electrode (SCE) as the reference electrode, and an Ni-based NW film as the working electrode. All the measurements were performed at room temperature and atmospheric pressure, in a one-compartment electrochemical Teflon cell filled with 100 mL of 1 M KOH (measured pH = 13.5) as the supporting electrolyte.

The potential distribution along the NW was numerically simulated by using COMSOL Multiphysics software.34 To simulate the NW electrode, a 20 nm thick NiO nanosheet was designed, while a bulk Au substrate was conceived as the current collector for the electrode. The following room temperature conductivities were used: 10−4 S cm−1 for NiO, 0.2 S cm−1 for 1 M KOH and an electrical permittivity of 11.9 for NiO.35,36 A steady-state model was used to evaluate the electric field distribution across the electrode at a constant applied voltage of 1.6 V.

X-ray photoelectron spectroscopy (XPS) analysis was used to investigate the oxidation state evolution of the NW before and after the OER. XPS spectra were recorded using an Al Kα photon source (1486.7 eV) and a hemispherical electron analyzer VG Microtech CLAM4 equipped with a multi-channeltron detector (MCD). The kinetic energy of the photoelectrons emitted from the sample surface was collected with a 20 eV pass energy, resulting in a line spectral resolution of about 1.2 eV. Au 4f7/2 was used as the calibration peak at 84.0 eV. The deconvolution and fitting of the peaks were carried out with fityk software.37

Results and discussion

The Ni(OH)2 and NiO NW were synthesized through a two-step process, as schematized in the top panel of Fig. 1. The first step involves CBD at 50 °C to ensure the growth of the Ni(OH)2 NW on top of the Au (50 nm)/Ti (25 nm)/quartz substrate. The second step consists of post-growth thermal annealing in Ar at 350 °C for 1 h, which induces dehydration of Ni(OH)2 into NiO. Fig. S1a (ESI) shows the SEM image of the pristine Ni(OH)2 NW film, which consists of a densely interconnected array of thin (∼20–30 nm) sheets mostly perpendicular to the substrate.18 The Ni(OH)2 NW film has a very high surface area of 30–40 m2 g−1, as measured previously by BET gas adsorption measurements.17 By increasing the synthesis time, the NW film thickness increases from 200 nm for 3 min, to 400 nm for 20 min growth time (Table S1 and Fig. S2, ESI). Notably, the morphology of the annealed NiO NW films does not appreciably change compared to the pristine Ni(OH)2 NW (Fig. S1, ESI), neither after the OER as shown in Fig. 1(a). In addition, EDX analysis, as shown in Fig. 1(b) and (c), confirmed that the NW composition is solely constituted by Ni and O. The EDX peaks of Au and Ti are ascribed to the underneath electrode substrate. Contamination of K from the electrolyte solution appears for samples after the electrochemical OER, while no traces of Fe were detected within the resolution of the EDX (<0.1%) as shown in the inset of Fig. 1(d), both before and after the OER (Fig. S3, ESI) analysis.
image file: d0ma00467g-f1.tif
Fig. 1 SEM image of the NiO NW (a) and the corresponding EDX-SEM colour map for Ni (b) and O (c) atomic signals, together with the EDX survey (d).

In order to measure the performances of the Ni(OH)2 and NiO NW electrocatalysts toward the OER, we performed a series of electrochemical measurements. In particular, each NW electrode was electrochemically characterized using the following series of tests: (1) electrochemical impedance spectroscopy (EIS); (2) cyclic voltammetry (CV); (3) EIS, (4) Tafel analysis (chronopotentiometry, CP); (5) EIS; (6) chronoamperometry (10 min); (7) CV and (8) the CP stability test for 5 h. The measured potential was converted to the overpotential, η′, against the reversible hydrogen electrode (RHE) according to the relationship:38,39

image file: d0ma00467g-t1.tif
where ERHE and ESCE are the potentials of the working electrode with respect to the RHE and the SCE, respectively. E0 is the standard reduction potential of the reference electrode with respect to the RHE, while R, T, and F are the gas constant, temperature, and Faraday constant. Moreover, the overpotential was also corrected for the uncompensated series resistance as follows:
η = η′ − iRu
where i is the current collected at the electrode, while Ru [Ohms] is the intercept on the real axis of the Nyquist plots (real vs. imaginary part of the impedance, Z) obtained from the EIS measurements performed in a frequency range between 1 Hz and 100 kHz at 0 V vs. open circuit potential (see Fig. S4 in the ESI).38

Fig. 2 shows the CV curves recorded for the Ni(OH)2 NW and for two different thicknesses of the NiO NW electrocatalyst. Two pronounced oxidation and reduction peaks appear for all the samples, which are attributed to the redox couple Ni2+/Ni3+. At higher values of overpotential, a strong increase of the current appears, due to the OER occurring at the electrocatalyst surface. In this regard, the pristine Ni(OH)2 NW electrode shows only moderate activity which is also accompanied by some electorcatalyst deterioration (Fig. S5, ESI). On the other side, the NiO NW electrocatalyst shows a higher current at a lower overpotential and increased stability. The latter is probably due to the increased stiffness of the NW film after calcination.


image file: d0ma00467g-f2.tif
Fig. 2 CV curves of Ni(OH)2 and NiO NW films deposited on Au/Ti/quartz substrates. All curves refer to the 10th cycle and the overpotential was corrected for the uncompensated resistance estimated from the EIS measurements.

It is important to remember that both NiO and Ni(OH)2 follow a similar redox reaction, which can be simplified with a single-electron reaction as:40,41

Ni(OH)2 + OH ↔ NiOOH + H2O + e
 
NiO + OH ↔ NiOOH + e(1)
Moreover, in Fe-free Ni oxides, NiOOH and especially its γ phase are often described as potential active electrocatalysts for the OER.42,43 In particular, γ-NiOOH has a layered structure consisting of NiOOH planes and intercalated water molecules or ions, with a larger interplanar distance than β-NiOOH.44,45 This results in a higher Ni oxidation state in γ-NiOOH (3.5–3.67) than in β-NiOOH (3), and thus in a superior catalytic activity.42 Such a peculiar structural characteristic is morphologically accompanied by the high surfaces exposed by our NW film, which is optimal to involve a larger amount of atoms in the OER process than bulky electrocatalyst films. Moreover, several studies have recently reported that minimal impurities of Fe were sufficient to improve the catalytic activity of Ni(OH)2,32,33 giving rise to an OER current of around 1 mA at 400 mV of overpotential. Although SEM-EDX and XPS analyses did not show any signal due to significant iron contamination both before and after electrochemical measurements, still Fe traces below the detection limit (<0.1%) cannot be completely excluded. However, we expect that the effect of such Fe contamination, if any, would be small and similar for all the investigated samples, keeping both the activity metrics and the latter discussion valid.

The stability of the NW electrodes was evaluated by running CP measurements with the electrodes kept at a current density of 10 mA cm−2 for five hours, while the overpotential changes were recorded. Fig. S6 (ESI) shows a different behavior between the NiO and Ni(OH)2 NWs. The Ni(OH)2 NW shows poor stability, with an overpotential stably increasing over time and exceeding the value of 420 mV after 5 h of OER activity. In contrast, the NiO NW films show an improved electrochemical stability, with both the 200 nm and the 400 nm thick NWs evidencing a nearly constant overpotential of around 345 mV and 350 mV, respectively. Similar to what was observed during the CV tests, such improved stability is probably related to a better stiffness of the NiO NW film compared to the bulk support electrode.

The different behavior observed in the CV and CP measurements between the NiO and Ni(OH)2 NW films is related to the different activities of the electrocatalysts towards the OER. To compare the activity of various electrocatalysts in water splitting, the overpotential at a current density of 10 mA cm−2 is often used.1,39 In this regard, as already clearly visible in Fig. 2 and 3, one can generally conclude that the NiO NW performs better than the Ni(OH)2 NW and the reaction becomes more effective when a thicker ∼400 nm NW electrocatalyst is used, since both the overpotential and stability are optimized. However, relying only on the values of the overpotential can be misleading since that is an intensive quantity and it is not quantitatively linked to the amount of active materials involved in the OER. For this reason, the steady-state Tafel equation was also used from the chronopotentiometry measurements to calculate the activity metrics. Generally, a smaller Tafel slope implies faster electrochemical kinetics.46,47 The Tafel slopes extrapolated from the linear fit of data points below 10 mA cm−2 are shown in Fig. 3(a). The Ni(OH)2 NW exhibits a slope of around 104 mV dec−1, while both the NiO NW electrodes exhibit a similar slope of around 50 mV dec−1. The lower slope of the NiO NW compared to that of the Ni(OH)2 NW might be related to a different OER process pathway. In fact, the Tafel slope around 120 mV dec−1 is typically observed when the reaction proceeds as M + OH → MOH + e, where M denotes the active site on the surface.47 However, when the surface has already some adsorbed OH species the reaction is found to proceed at a lower Tafel slope, typically around 30–40 mV dec−1.47 In this regard, it was recently shown that the increased electrochemical kinetics of the NiOx structures compared to that of Ni(OH)2 is related to an increased amount of oxygen vacancies and point defects, favouring the adsorption of hydroxide groups and driving the OER at a lower energy rate step.15,40,42 This would lead to a more favourable formation of NiOOH complexes at the electrocatalyst surface and to a more effective OER process. Moreover, the better stiffness of the NiO NW might help in improving the electrochemical stability of the entire film at a high current density.


image file: d0ma00467g-f3.tif
Fig. 3 Steady-state Tafel plots (a) and turn-over frequency (TOF) curves (b) of Ni(OH)2 and NiO NWs films. The values of the overpotential for Tafel analysis were acquired from CP measurements in steps from 0.05 mA cm−2 to 10 mA cm−2, each held for 3 min. The TOF values were calculated considering the number of active sites extracted from electrochemical measurements (TOFredox), or measured by QCM (TOFQCM).

To shed more light on the different activities between the Ni(OH)2 and NiO NW films, we also extracted more quantitative information on the amount of electrocatalysts participating in the OER by analysing the oxidation peak in the CV curves. As shown in Fig. 2, a clear difference among the investigated samples appears in the intensity of the redox peaks, which is intimately related to a different electro-catalytic activity. In fact, the area underneath the peak is proportional to the amount of active electrocatalytic sites available for the OER process.39,48 The current i recorded during CV is a measure of the charge Q passed over a period of time: image file: d0ma00467g-t2.tif. Given that the current sweep is acquired at a given scan rate, image file: d0ma00467g-t3.tif, the integration of the current peak returns the amount of charge passed through the electrode during the redox reaction. This relationship is valid with the assumption that the redox reaction is a one-electron transfer process as written in reaction (1). In our case, the Ni(OH)2 NW electrode exhibits the smallest area of the peak, corresponding to an amount of 1.7 × 1017 active sites per cm2. Instead, the NiO NW has an amount of active sites increasing from 2.8 × 1017 sites per cm2 (200 nm) to 5.6 × 1017 sites per cm2 (400 nm), as reported in Table 1.

Table 1 Activity metrics of Ni(OH)2 and NiO NW electrocatalysts
Ni(OH)2_200 nm NiO_200 nm NiO_400 nm
Overpotential at 10 mA cm−2 [mV] 420 345 350
Tafel slope [mV dec−1] 104 48 52
Number of active sites [×1017 cm−2] 1.7 2.8 5.6
Total active electrocatalyst [μmol cm−2] 0.28 0.46 0.91
Fraction of active electrocatalyst [±10%] 80% ∼100% 57%
Current density at η = 350 mV [A cm−2] 7.05 × 10−3 20.1 × 10−3 28.5 × 10−3
TOF at η = 350 mV [s−1] 9.7 × 10−2 1.8 × 10−1 8.1 × 10−2


The number of active electrocatalytic sites determined from the electrochemical measurements is in good agreement with the total density of the electrocatalyst, as obtained from the QCM measurements and reported in Table S1 (ESI). In particular, for both the 200 nm samples, the number of active electrocatalysts closely matches with that obtained by QCM. This means that nearly all atoms participate in the OER process, confirming that the nanostructures are effective for material utilization. In fact, the porous-like 3D morphology of our NW thin films is of great help for optimizing the amount of electrocatalysts ionically connected to the OH groups and electronically connected to the current collector. Nonetheless, it is worth noting that the thicker NiO NW has a lower fraction of active electrocatalysts, suggesting limited effectiveness of the OER process. To better investigate the metrics relevant to the intrinsic activity of the electrocatalysts in the OER, the turn-over frequency (TOF) must be considered.4 The TOF is defined as the rate of production of oxygen molecules per available (and active) site:

image file: d0ma00467g-t4.tif
where I is the measured current at a certain overpotential, F is the Faraday constant (96[thin space (1/6-em)]485 C mol−1) and n is the number of moles of the available (active) sites determined by QCM (TOFQCM) or by the redox peak integration (TOFredox). It should be noted that, unfortunately, the literature data are usually biased towards the record activity claiming and often discarding the amount of available sites and the activity of each catalytic site.4 The TOFQCM and TOFredox are extremely useful metrics for determining the activity of each site, even if on an average scale, considering the full electrocatalyst loading or the redox active one, respectively. A higher TOF is desirable since each available site produces more O2 molecules per unit time, as well as a convergence between TOFQCM and TOFredox is wished for better material utilization. Fig. 3(b) shows the trends of the TOFQCM and TOFredox values in the 300–400 mV overpotential range. Clearly, the TOF increases with the applied overpotential for kinetics reasons, and still the number of active sites really matters for defining the effectiveness of the OER process. The 200 nm-thin NiO NW film always shows higher values of TOF and a nice convergence of TOFQCM and TOFredox, meaning that on average all the active sites are available to activate an effective OER. As reported in Table 2, a TOF of 0.18 s−1 is obtained at 350 mV of overpotential. Although the Ni(OH)2 NW film has a fraction of active electrocatalyst comparable to that of the 200 nm-thin NiO NW film, its TOF values are systematically lower as demonstrated by its minor OER current. Increasing the thickness of the NiO NW film leads to an expected increase of the current density, but still the material utilization decreases as shown by the considerably reduced TOF. Such behavior reveals that increasing the thickness of the NW film does not always lead to a corresponding increase of the intrinsic OER performance, because of the lower percentage of the active electrocatalyst. In the thicker NW, the electrochemical properties are somehow weakened, leading to less effective material utilization. The highest mass activity has been found for the 200 nm thin NiO NW film with a remarkable value of 0.33 A mg−1 at a current of 10 mA cm−2 with an overpotential of 345 mV. The measured activity metrics of all our samples are considerably higher, or among the highest performances reported in the literature for NiO based electrocatalysts, as shown in Table 2. Indeed, our NiO NW electrocatalyst shows the best combination because of its low values of overpotential and Tafel slope and a high TOF.

Table 2 Activity metrics of NiO based electrocatalysts for the OER
Electrocatalyst material Electrolyte Overpotential (mV) at 10 mA cm−2 Tafel slope (mV dec−1) TOF (s−1) at η = 350 mV Electrode Ref.
NiO hollow nanofibers 1 M KOH 322 78 0.07 Ni foam 49
α-Ni(OH)2 nanospheres 0.1 M KOH 331 42 0.036 Glassy carbon 50
NiTi oxide nanosheets 1 M KOH 320 52 0.005 Glassy carbon 51
NiO nanowalls 1 M KOH 310 54 NA Nickel foam 52
NiO thin films 0.5 M KOH 360 30 0.07 ITO 53
Ni(OH)2 nanoplates 0.1 M KOH 474 87 0.015 (at 490 mV) ITO 54
Ni/NiO nanoparticles 1 M KOH 320 61 0.11 Glassy carbon 55
NiOx films 1 M KOH 380 42 NA Glassy carbon 56
NiO nanosheets 0.1 M KOH 422 116 NA Carbon cloth 57
NiO nanosheets 1 M KOH 320 52 NA Graphene 58
NiO nanowalls 1 M KOH 345 48 0.18 Quartz/Ti/Au This work


In order to study the origin of the higher activity for the smaller NiO NW, the electric potential field distribution along the NW electrode during the electrochemical activity was simulated by using the COMSOL Multiphysics software. The simulation on such a macroscopic quantity can offer a valuable understanding of the basic processes occurring at the nanoscale. The results of the applied potential distribution across the NW are presented in Fig. 4 in a false colour scale from 1.3 to 1.6 V. The 200 nm-thin NW displays a nearly uniform potential field along its structure, with a minimal potential decrease, lower than 0.1 V, near the top region of the NW. By doubling the NW length, a considerably larger potential decrease is observed, with a NW tip at a potential 0.3 V below the Au contact. This effect is detrimental for the OER since only a portion of the material is at a potential high enough to achieve the electrochemical reaction. This effect helps explain the reduced activity metrics evaluated for the thicker NW film electrodes. Only the region close to the NW–substrate interface experiences a potential high enough to efficiently drive the OER process. On the top region of the longer NW, the potential field is reduced to a level close to the thermodynamic limit for the OER of 1.23 eV, for which the reactions can only poorly occur.


image file: d0ma00467g-f4.tif
Fig. 4 Electric potential distribution in the NiO NW electrodes with different NW sizes in 1 M KOH solution for 1.6 V of applied bias, as simulated by the COMSOL Multiphysics software. A 20 nm thick and 200 (or) 400 nm tall NiO nanosheet was used to simulate the NiO NW electrodes.

Finally, to compare the OER activity of the NiO NW with the chemical evolution at the electrode surface, we performed XPS analysis on the 400 nm-thick NiO NW film electrode before and after the OER. In particular, for the NiO NW electrode we ran a CP test at 10 mA cm−2 for 1 h just before introducing it into the XPS analysis chamber. This was done with the intention of verifying whether the lower TOF estimated thicker NW film is related to incomplete chemical transformation of the electrocatalyst and to the presence of an inert material.

Fig. 5 shows the Ni 2p3/2 and O 1s spectra of the NiO NW before and after the OER. The quantification and interpretation of the XPS peak shape of the Ni-based oxides are not trivial, due to the presence of extended multiplets, shake-up and plasmon loss structures, which can be confused with the overlapping of different chemical states of Ni.59–61 For the XPS data fitting, the extensive study done by Biesinger et al. was used as a guideline.60 They concluded that the full Ni 2p photoemission envelope for pure Ni2+ species (e.g., NiO or Ni(OH)2) and pure Ni3+ species (e.g., γ-NiOOH) can be fit with a unique set of seven components.60,61 The binding energies, peak distances and FWHM were kept fixed in our fitting, according to the values given by Biesinger et al.,60 while only the peak intensities were used as free parameters. The fit values are summarized in Table S2 of the ESI.


image file: d0ma00467g-f5.tif
Fig. 5 XPS spectra of the 400 nm thick NiO NW electrocatalyst. Ni 2p3/2 (a) and O 1s (b) for the NiO NW before the OER. Ni 2p3/2 (c) and O 1s (d) for the NiO NW after the OER.

Fig. 5(a) shows the Ni 2p3/2 spectra of the NiO NW before the OER (as annealed). The broad peak in the range between 852 and 858 eV is due to the overlap of the NiO component (the main peak at 853.6 eV and the multiplet at 855.2 eV) with the Ni(OH)2 multiplet peaks, while the broad shoulder between 858 and 868 eV is due to the satellite peaks of NiO and Ni(OH)2. The presence of peaks related to the Ni(OH)2 states in the NiO films is not unexpected, since hydroxide groups can readily adsorb on the surface because of ambient moisture.58 Interestingly, the same information also comes from the O 1s peak shown in Fig. 5(b), where the peak at 529.6 eV is related to the Ni–O bond and is accompanied by a peak at 531.1 due to Ni(OH)2, together with an adventitious contamination peak at 532 eV and water adsorbates at around 533.3 eV. From both the Ni 2p and O 1s spectra, the ratio of the intensities of the components related to the Ni(OH)2 and NiO peaks (see Table S2 in the ESI) indicates that about 40% of the Ni atoms in the NiO NW film before the OER is actually in the chemical state of Ni(OH)2. Therefore, it is reasonable to assume that the freshly annealed NiO NW has a thin shell of Ni(OH)2 of a few nm surrounding the NiO core. The presence of such a bimodal chemical composition of Ni atoms is maintained also in the Ni 2p and O 1s XPS spectra of the NW electrode after the OER, as shown in Fig. 5(c) and (d). The presence of NiO is confirmed by the peak at 853.5 eV for Ni 2p3/2 and at 529.5 eV for the O 1s spectra. However, as especially evident from the O 1s spectrum, a larger signal comes from the Ni3+ species due to the presence of NiOOH. From the quantitative analysis of the intensities of the peaks related to NiO and NiOOH, it is possible to estimate that NiOOH constitutes only about 60% of the overall composition of the NW electrode after the OER. Such a value is further confirmation that around 40% of the total amount of atoms, an amount that is not negligible, does not follow the redox reaction and is not active towards the OER in the thick NW film. Such an amount of inert atoms is perfectly in agreement with the estimation of the inactive electrocatalyst in the electrochemical activity metrics and in conceptual agreement with the large potential decrease calculated for the 400 nm-thick NW film.

Thus, for the design of novel Ni-based electrocatalysts, one should focus on optimizing the thickness of the electrocatalysts and increasing the amount of available electrocatalytic sites by increasing the total surface area, instead of indefinitely increasing the thickness and the mass loading only.

Conclusions

We performed a quantitative investigation of the OER process in highly textured Ni(OH)2 and NiO NW films, synthesized by low-cost methods. Electrochemical measurements revealed that, in comparison to Ni(OH)2, the NiO NW film shows a significant improvement in the OER performance, with an overpotential of 345 mV and a Tafel slope as low as 48 mV dec−1. The noteworthy performances of the NiO NW are also supported by its high activity metrics, in terms of a mass activity up to 0.33 A mg−1 and a TOF value of 0.18 s−1 at 350 mV overpotential. By comparing the NiO NW at different lengths, electrochemical measurements showed that a lower percentage of active sites is found, bringing down the overall OER performance. Nearly all the available sites are active in a 200 nm long NW, while in a longer 400 nm NW less than 60% of the electrocatalyst is involved in the OER. A numerical simulation of the electrical potential distribution and a detailed XPS analysis confirm that a large part of NiO in the longer NW films remains in an inert chemical state, probably because a lower electric potential is experienced. Such results contribute towards building a solid understanding of the OER mechanism in Ni-based nanostructures, and can help in defining a roadmap for material optimization in nanostructured electrocatalysts.

Conflicts of interest

All authors contributed to the final version of this paper. The authors declare that there is no conflict of interest regarding the publication of this article.

Acknowledgements

Sergio Battiato aknowledges the project AIM1804097 – Programma Operativo Nazionale FSE –FESR “Ricerca e Innovazione 2014–2020”, Mario Urso aknowledges the project PON MIUR ADAS+ (ARS01_00459).

References

  1. I. Roger, M. A. Shipman and M. D. Symes, Nat. Rev. Chem., 2017, 1(1), 1–13 CrossRef.
  2. J. Rongé, T. Bosserez, D. Martel, C. Nervi, L. Boarino, F. Taulelle, G. Decher, S. Bordiga and J. A. Martens, Chem. Soc. Rev., 2014, 43, 7963–7981 RSC.
  3. A. Landman, H. Dotan, G. E. Shter, M. Wullenkord, A. Houaijia, A. Maljusch, G. S. Grader and A. Rothschild, Nat. Mater., 2017, 16(6), 646–651 CrossRef CAS PubMed.
  4. J. Kibsgaard and I. Chorkendorff, Nat. Energy, 2019, 4(6), 430–433 CrossRef.
  5. J.-W. Wang, W.-J. Liu, D.-C. Zhong and T.-B. Lu, Coord. Chem. Rev., 2019, 378, 237–261 CrossRef CAS.
  6. T. Hisatomi, K. Takanabe and K. Domen, Catal. Lett., 2015, 145(1), 95–108 CrossRef CAS.
  7. S. Chen, S. S. Thind and A. Chen, Electrochem. Commun., 2016, 63, 10–17 CrossRef CAS.
  8. X. Li, X. Hao, A. Abudula and G. Guan, J. Mater. Chem. A, 2016, 4(31), 11973–12000 RSC.
  9. A. Shinde, D. Guevarra, J. A. Haber, J. Jin and J. M. Gregoire, J. Mater. Res., 2015, 30(3), 442–450 CrossRef CAS.
  10. X. Zou and Y. Zhang, Chem. Soc. Rev., 2015, 44(15), 5148–5180 RSC.
  11. M. S. Burke, L. J. Enman, A. S. Batchellor, S. Zou and S. W. Boettcher, Chem. Mater., 2015, 27(22), 7549–7558 CrossRef CAS.
  12. J. B. Gerken, S. E. Shaner, R. C. Massé, N. J. Porubsky and S. S. Stahl, Energy Environ. Sci., 2014, 7(7), 2376–2382 RSC.
  13. B. Zhang, X. Zheng, O. Voznyy, R. Comin, M. Bajdich, M. García-Melchor, L. Han, J. Xu, M. Liu, L. Zheng, F. P. G. de Arquer, C. T. Dinh, F. Fan, M. Yuan, E. Yassitepe, N. Chen, T. Regier, P. Liu, Y. Li, P. De Luna, A. Janmohamed, H. L. Xin, H. Yang, A. Vojvodic and E. H. Sargent, Science, 2016, 352(6238), 333–337 CrossRef CAS PubMed.
  14. D. Friebel, M. W. Louie, M. Bajdich, K. E. Sanwald, Y. Cai, A. M. Wise, M.-J. Cheng, D. Sokaras, T.-C. Weng, R. Alonso-Mori, R. C. Davis, J. R. Bargar, J. K. Nørskov, A. Nilsson and A. T. Bell, J. Am. Chem. Soc., 2015, 137(3), 1305–1313 CrossRef CAS PubMed.
  15. Q. Hu, X. Huang, Z. Wang, G. Li, Z. Han, H. Yang, X. Ren, Q. Zhang, J. Liu and C. He, J. Mater. Chem. A, 2020, 8(4), 2140–2146 RSC.
  16. Y. Li, X. Bao, D. Chen, Z. Wang, N. Dewangan, M. Li, Z. Xu, J. Wang, S. Kawi and Q. Zhong, ChemCatChem, 2019, 11(24), 5913–5928 CrossRef CAS.
  17. K. O. Iwu, A. Lombardo, R. Sanz, S. Scirè and S. Mirabella, Sens. Actuators, B, 2016, 224, 764–771 CrossRef CAS.
  18. M. Urso, G. Pellegrino, V. Strano, E. Bruno, F. Priolo and S. Mirabella, Nanotechnology, 2018, 29(16), 165601 CrossRef CAS PubMed.
  19. M. Urso, S. G. Leonardi, G. Neri, S. Petralia, S. Conoci, F. Priolo and S. Mirabella, Sens. Actuators, B, 2020, 305, 127481 CrossRef.
  20. T. P. Mokoena, H. C. Swart and D. E. Motaung, J. Alloys Compd., 2019, 805, 267–294 CrossRef CAS.
  21. X. H. Xia, J. P. Tua, J. Zhang, X. L. Wang, W. K. Zhang and H. Huang, Sol. Energy Mater. Sol. Cells, 2008, 92(6), 628–633 CrossRef CAS.
  22. M. Urso, G. Torrisi, S. Boninelli, C. Bongiorno, F. Priolo and S. Mirabella, Sci. Rep., 2019, 9, 7736 CrossRef PubMed.
  23. H. Lai, Q. Wu, J. Zhao, L. Shang, H. Li, R. Che, Z. Lyu, J. Xiong, L. Yang, X. Wanga and Z. Hu, Energy Environ. Sci., 2016, 9(6), 2053–2060 RSC.
  24. J. Zheng, W. Zhou, T. Liu, S. Liu, C. Wang and L. Guo, Nanoscale, 2017, 9(13), 4409–4418 RSC.
  25. M. Schalenbach, F. D. Speck, M. Ledendecker, O. Kasian, D. Goehl, A. M. Mingers, B. Breitbach, H. Springer, S. Cherevko and K. J. J. Mayrhofer, Electrochim. Acta, 2018, 259, 1154–1161 CrossRef CAS.
  26. T. Wang, R. Jin, X. Wu, J. Zheng, X. Li and K. Ostrikov, J. Mater. Chem. A, 2018, 6(19), 9228–9235 RSC.
  27. P. Jiang, Q. Liu and X. Sun, Nanoscale, 2014, 6(22), 13440–13445 RSC.
  28. G. B. Darband, M. Aliofkhazraei, S. Hyun, A. S. Rouhaghdam and S. Shanmugam, Nanoscale, 2019, 11(35), 16621–16634 RSC.
  29. X. Meng, J. Han, L. Lu, G. Qiu, Z. L. Wang and C. Sun, Small, 2019, 15(41), 1902551 CrossRef CAS PubMed.
  30. M. K. Bates, Q. Jia, H. Doan, W. Liang and S. Mukerjee, ACS Catal., 2016, 6(1), 155–161 CrossRef CAS.
  31. G. Huang, R. Fan, X. Zhou, Z. Xu, W. Zhou, W. Dong and M. Shen, Chem. Commun., 2019, 55(3), 377–380 RSC.
  32. I. Roger and M. D. Symes, J. Am. Chem. Soc., 2015, 137(43), 13980–13988 CrossRef CAS PubMed.
  33. L. Trotochaud, S. L. Young, J. K. Ranney and S. W. Boettcher, J. Am. Chem. Soc., 2014, 136(18), 6744–6753 CrossRef CAS PubMed.
  34. COMSOL Multiphysics® v. 5.3. http://www.comsol.com. COMSOL AB, Stockholm, Sweden.
  35. R. J. Gilliam, J. W. Graydon, D. W. Kirk and S. J. Thorpe, Int. J. Hydrogen Energy, 2007, 32(3), 359–364 CrossRef CAS.
  36. A. Motori and F. Sandrolini, J. Power Sources, 1994, 48(3), 361–370 CrossRef CAS.
  37. https://fityk.nieto.pl .
  38. L. Geerts, S. Cosentino, T.-W. Liao, A. Yadav, P.-C. Lin, V. S. Zharinov, K.-J. Hu, A. Longo, L. M. C. Pereira, D. Grandjean, J. Rongé, P. Lievens and J. A. Martens, Catal. Today, 2019, 334, 59–67 CrossRef CAS.
  39. M. B. Stevens, L. J. Enman, A. S. Batchellor, M. R. Cosby, A. E. Vise, C. D. M. Trang and S. W. Boettcher, Chem. Mater., 2017, 29(1), 120–140 CrossRef CAS.
  40. E. Arciga-Duran, Y. Meas, J. J. Perez-Bueno, J. C. Ballesteros and G. Trejo, Electrochim. Acta, 2018, 268, 49–58 CrossRef CAS.
  41. V. C. Hoang, K. N. Dinh and V. G. Gomes, Carbon, 2020, 157, 515–524 CrossRef CAS.
  42. O. D. Morales, D. F. Suspedra and M. T. M. Koper, Chem. Sci., 2016, 7(4), 2639–2645 RSC.
  43. Z. Xue, X. Zhang, J. Qin and R. Liu, J. Mater. Chem. A, 2019, 7(40), 23091–23097 RSC.
  44. P. Oliva, J. Leonardi, J. F. Laurent, C. Delmas, J. J. Braconnier, M. Figlarz and A. D. Guibert, J. Power Sources, 1982, 8, 229–255 CrossRef CAS.
  45. D. G. Evans and R. C. Slade, Layered double hydroxides, Springer, 2006, pp. 1–87 Search PubMed.
  46. B. Wang, C. Tang, H.-F. Wang, X. Chen, R. Cao and Q. Zhang, Adv. Mater., 2019, 31(4), 1805658 CrossRef PubMed.
  47. T. Shinagawa, A. T. Garcia-Esparza and K. Takanabe, Sci. Rep., 2015, 5, 13801 CrossRef PubMed.
  48. S. Trasatti, Electrochim. Acta, 1991, 36(2), 225–241 CrossRef CAS.
  49. V. D. Silva, T. A. Simones, J. P. F. Grilo, E. S. Medeiros and D. A. Macedo, J. Mater. Sci., 2020, 55(15), 6648–6659 CrossRef CAS.
  50. M. Gao, W. Sheng, Z. Zhuang, Q. Fang, S. Gu, J. Jiang and Y. Yan, J. Am. Chem. Soc., 2014, 136(19), 7077–7084 CrossRef CAS PubMed.
  51. Y. Zhao, X. Jia, G. Chen, L. Shang, G. I. N. Waterhouse, L.-Z. Wu, C.-H. Tung, D. O’Hare and T. Zhang, J. Am. Chem. Soc., 2016, 138(20), 6517–6524 CrossRef CAS PubMed.
  52. P. T. Babar, A. C. Lokhande, M. G. Gang, B. S. Pawar, S. M. Pawar and J. H. Kim, J. Ind. Eng. Chem., 2018, 60, 493–497 CrossRef CAS.
  53. A. C. Pebley, E. Decolvenaere, T. M. Pollock and M. J. Gordon, Nanoscale, 2017, 9(39), 15070–15082 RSC.
  54. X. Zhou, Z. Xia, Z. Zhang, Y. Ma and Y. Qu, J. Mater. Chem. A, 2014, 2(30), 11799–11806 RSC.
  55. F. E. S. Oztuna, T. Beyazay and U. Unal, J. Phys. Chem. C, 2019, 123(46), 28131–28141 CrossRef.
  56. L. Tong, W. Wu, K. Kuepper, A. Scheurer and K. Meyer, ChemSusChem, 2018, 11(16), 2752–2757 CrossRef CAS PubMed.
  57. N. Cheng, Q. Liu, J. Tian, X. Sun, Y. He, S. Zhai and A. M. Asiri, Int. J. Hydrogen Energy, 2015, 40(32), 9866–9871 CrossRef CAS.
  58. W. Yuan, C. Li, M. Zhao, J. Zhang, C. M. Li and S. P. Jiang, Electrochim. Acta, 2020, 342, 136118 CrossRef CAS.
  59. A. Scandurra, A. Porto, L. Mameli, O. Viscuso, V. Del Bo and S. Pignataro, Surf. Interface Anal., 1994, 22(1–12), 353–357 CrossRef CAS.
  60. M. C. Biesinger, B. P. Payne, L. W. M. Lau, A. Gerson and R. St. C. Smart, Surf. Interface Anal., 2009, 41(4), 324–332 CrossRef CAS.
  61. A. P. Grosvenor, M. C. Biesinger, R. St. C. Smart and N. S. McIntyre, Surf. Sci., 2006, 600(9), 1771–1779 CrossRef CAS.

Footnotes

Electronic supplementary information (ESI) available. See DOI: 10.1039/d0ma00467g
These two authors contributed to this work equally.

This journal is © The Royal Society of Chemistry 2020
Click here to see how this site uses Cookies. View our privacy policy here.