Yuanxing
Yun
a,
Jie
Shao
*ac,
Xuefang
Shang
b,
Wei
Wang
ad,
Weibo
Huang
a,
Qunting
Qu
*ad and
Honghe
Zheng
*ad
aCollege of Energy, Soochow Institute for Energy and Materials InnovationS, Soochow University, Suzhou, Jiangsu 215006, China. E-mail: qtqu@suda.edu.cn; hhzheng@suda.edu.cn; shaojie@suda.edu.cn
bKey Laboratory of Medical Molecular Probes, School of Basic Medical Sciences, Xinxiang Medical University, Jinsui Road 601, Xinxiang, Henan 453003, China
cCollege of Chemistry, Chemical Engineering and Material Science, Soochow University, Suzhou, Jiangsu 215006, China
dSuzhou Huaying New Energy Materials and Technology Co., Ltd., Suzhou, Jiangsu 215100, China
First published on 25th February 2020
To obtain an electrode material that is capable of manifesting high Na-ion storage capacity during long-term cycling at a rapid discharge/charge rate, ternary heterophases MoSe2/MoO2/carbon are rationally designed and synthesized through a supermolecule-assisted strategy. Through using supermolecules that are constructed from MoO42− and polydopamine as the precursor and sulfonated polystyrene microspheres as the sacrificial template, the in situ formed ternary phases MoSe2/MoO2/carbon are fabricated into a hollow microspherical structure, which is assembled from ultrathin nanosheets with MoSe2 and MoO2 nanocrystallites strongly embedded in a nitrogen-doped carbon matrix. In the ternary phases, the MoSe2 phase contributes to a high Na-ion storage capacity by virtue of its layered crystalline structure with a wide interlayer space, while the surrounding MoO2 and porous nitrogen-doped carbon phases are conducive to rate behaviour and cycling stability of the ternary hybrids since both the two phases are beneficial for electronic transport and structural stability of MoSe2 during repeated sodiation/desodiation reaction. The as-prepared MoSe2/MoO2/carbon manifests excellent rate behaviour (a Na-ion storage capacity of 461 mA h g−1 at an extremely high current density of 70 A g−1) and outstanding cycle performance (610 mA h g−1 after 1000 cycles).
Besides the rate behavior, MoSe2 is confronted with the issue of poor cycling stability when being used as the anode material of SIBs.8 On the one hand, MoSe2 as a typical two-dimensional material is most commonly fabricated into a nanosheet-like structure, which tends to restack or aggregate during repeated sodiation/desodiation, leading to gradual loss of active sites.24 On the other hand, the as-formed Na2Se after the first sodiation process could not be completely recovered to the MoSe2 phase and might be converted to Se element in the subsequent desodiation reaction.9,25–27 Thus the electrochemical mechanism of MoSe2 after the first cycle would be analogous to those of sulfur or selenium-based cathodes in Li–S, Li–Se or Na–Se batteries involving the conversion reactions of S to Li2S, Se to Li2Se, or Se to Na2Se, respectively. For these batteries, the formation of soluble polyselenide/polysulfide intermediates always leads to a severe shuttle effect and rapid capacity degradation during discharge/charge.28,29 Various porous carbons and transition metal oxides have been adopted for physical or chemical confinement to prevent polyselenide/polysulfide dissolution from sulfur or selenium-based cathodes and improve the cycling performance of these batteries.30–33 By analogy to these sulfur or selenium-based cathodes, the combination of MoSe2 with carbons or transition metal oxides is also expected to bring about improved cycling stability of MoSe2 for Na-ion storage.
With these backgrounds, this work proposes a supermolecule-assisted strategy to synthesize embedding-type structured ternary heterophases MoSe2/MoO2/carbon. Through the incomplete selenization of Mo-based oxides during pyrolysis of MoO42−-polydopamine (Mo-PDA) supermolecules, the ternary heterophases with MoSe2 and MoO2 nanoparticles uniformly embedded in a carbon matrix are obtained. Compared to the totally selenized binary phases MoSe2/carbon and unselenized binary phases MoO2/carbon, the ternary phases MoSe2/MoO2/carbon exhibit significantly improved Na-ion storage performance. By virtue of the superior Na-ion storage capability of MoSe2, good electronic conductivity of MoO2 and carbon, and the unique embedding-type structure in which the surrounding MoO2 and carbon phases can preserve the structural stability of MoSe2, the ternary heterophases exhibit excellent rate behavior (a Na-ion storage capacity of 461 mA h g−1 at an extremely high current density of 70 A g−1) and outstanding long-term cycling performance, maintaining a capacity of 610 mA h g−1 after 1000 cycles.
Fig. 1 Schematic illustration of the synthesis procedure of hollow microspherical MoSe2/MoO2/carbon ternary phases. |
Scanning electron microscopy (SEM) images of the intermediate SPS@Mo–PDA and end product MoSe2/MoO2/NC are shown in Fig. 2. The morphology of SPS@Mo-PDA (Fig. 2a) exhibits the same microspherical structure to that of the original SPS template. Compared to the smooth surface of pure SPS (Fig. S3†), nanosheet-like Mo-PDA is obviously grown on the surface of microspheres. After pyrolysis and selenization, the microspherical morphology is perfectly maintained, and the 2D nanosheet-like structure becomes more distinct due to the formation of crystalline-state MoSe2/MoO2/NC (Fig. 2b–d). The MoSe2/MoO2/NC microspheres possess a homogeneous diameter of around 600 nm. No extra particles or uneven aggregates are observed, suggesting that Mo-PDA supermolecules preferentially grow on the surface of SPS, which guarantees the homogeneous microspherical morphology of the product. In addition, a hollow interior is supposed to be formed in these microspheres since some holes as indicated by the red arrows in Fig. 2d are distinguishable.
The hollow interior of MoSe2/MoO2/NC microspheres is also clearly observed through transmission electron microscopy (TEM). As shown in Fig. 3a, the black edges are in sharp contrast to the grey central areas, and the walls of the hollow microspheres are composed of ultrathin nanosheets. From the high-resolution TEM images (Fig. 3b and S4†), the lattice fringes with interplanar spacings of 0.28 and 0.65 nm are easily found, which can be indexed to the (100) and (002) crystalline planes of MoSe2, respectively. The lattice fringes with an interplanar spacing of 0.20 nm correspond to the (200) crystalline planes of MoO2. Besides MoSe2 and MoO2 crystallites, some porous and undefined regions, which should be amorphous carbon, are distributed in the hybrid. The dimensions of MoSe2 and MoO2 crystallites are observed to be less than 5 nm, so the structure of the ternary hybrid is described as ultrasmall MoSe2 and MoO2 crystallites embedded in a carbon matrix, which is the typical structure of supermolecule-derived materials. During the preparation of the ternary MoSe2/MoO2/NC hybrid, the PDA-derived carbon plays the role of restricting the growth of MoSe2 and MoO2, thereby giving rise to the formation of ultrasmall MoSe2 and MoO2 crystallites. Moreover, the in situ formation of N-doped carbon and MoSe2/MoO2 through the use of the Mo-PDA precursor could generate a strong interfacial interaction among the neighbouring phases, which is beneficial for Li-ion and electron transfer across the interface.
Fig. 3 (a) TEM and (b) high-resolution TEM images, (c) EDS elemental mapping images and (d) EDS linear scan profiles of hollow microspherical MoSe2/MoO2/NC ternary phases. |
The elemental mapping images (Fig. 3c) of the hybrid obtained through energy dispersive X-ray spectroscopy (EDS) confirm the coexistence of Mo, Se, O, C, and N elements, which are homogeneously distributed in the wall of hollow microspheres. The linear scan profiles of all the elements along the diameter of one typical microsphere (Fig. 3d) exhibit double peaks on both sides with the lowest intensity in central areas, which further demonstrate the hollow microspherical structure of the ternary hybrid. The Brunauer–Emmett–Teller (BET) surface area of MoSe2/MoO2/NC determined by N2 adsorption/desorption isotherms (Fig. S5†) is 190 m2 g−1. Such a high surface area should originate from the porous carbon and hollow microspherical structure of the hybrid phase as observed from TEM images.
The crystalline phases of the product were further investigated using X-ray diffraction (XRD). As shown in Fig. 4a, the diffraction peaks can be well indexed to the hybrid phases of hexagonal 2H-MoSe2 (JCPDS no. 29-0914) and monoclinic MoO2 (JPCDS no. 32-0671).39,40 Besides the typical peaks characteristic of MoSe2, several weak diffraction peaks at 26.0°, 36.8° and 53.5° are well consistent with standard peaks of MoO2, further validating the presence of MoO2 in the composite. Notably, all the XRD peaks of MoSe2/MoO2/NC are quite weak or broad, which is ascribed to the ultrasmall size of MoSe2 and MoO2 nanocrystallites. There are no obvious peaks characteristic of graphitic carbon, suggesting that the carbon derived from the organic ligands of Mo-PDA is mainly amorphous. Raman spectroscopy was used to further ascertain the presence of carbon and also verify the hybrid crystalline phases of MoSe2/MoO2/NC. As shown in Fig. 4b, the two characteristic peaks of carbon, D-band and G-band, appear at 1353 and 1580 cm−1, respectively. Besides, the two peaks at around 237 and 287 cm−1 correspond to the out-of-plane A1g and in-plane E12g modes of MoSe2,41 while other peaks at 492, 573 and 745 cm−1 are characteristic of MoO2.42
Fig. 4 (a) XRD patterns and (b) Raman spectra of MoSe2/MoO2/NC, and (c and d) the deconvoluted XPS spectra in the core-level regions of Mo 3d and N 1s. |
X-ray photoelectron spectroscopy (XPS) was used to investigate the surface electronic state of each of the elements in the ternary phases MoSe2/MoO2/carbon. The survey spectrum reveals the existence of Mo, Se, O, C, and N elements (Fig. S6†). The deconvoluted spectra of the Mo 3d core level are shown in Fig. 4c. The doublet peaks at the binding energies of 231.5 and 228.3 eV can be attributed to the Mo 3d3/2 and Mo 3d5/2 spin-orbits of Mo4+ in the environment of MoSe2, while the neighboring doublet peaks at slightly higher binding energies of 232.4 eV and 229.2 eV signify the presence of MoO2.13,42,43 The one broad peak at a binding energy of around 234 eV usually originates from the slight oxidation of Mo4+ to Mo6+ when the sample is exposed to air.13 The deconvoluted satellite peaks at lower binding energies of 230.4 and 227.5 eV can be indexed to the Mo–N bond, the formation of which results from the incorporation of nitrogen into the hybrids through the use of a N-containing supermolecule precursor. The XPS spectrum of the Se 3d core level is split into two peaks at 54.9 and 53.8 eV, corresponding well with the Se 3d3/2 and Se 3d5/2 spin-orbits of Se2− (Fig. S7†).42 The deconvoluted XPS spectra of the C 1s core level (Fig. S8†) exhibit one dominant peak at 284.6 eV, which is characteristic of carbon materials. The deconvoluted XPS spectra in the core level region of N 1s are shown in Fig. 4d. The two binding energies at 398.8 and 401.1 eV can be identified as pyridinic-N and graphitic-N species located at the six-member ring of the carbon lattice. One additional peak at 396.5 eV can be attributed to the Mo–N bond.
To gain insight into the differences between the electronic states of Mo element in MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC, XPS spectra of binary MoO2/NC and MoSe2/NC in the core-level region of Mo 3d were also measured and are shown in Fig. S9 and S10,† respectively. In the case of binary MoO2/NC, the binding energies of 230.0 and 232.9 eV can be assigned to Mo4+ species, while the binding energies of 231.8 and 235.0 eV signify the presence of Mo6+. The relatively high content of Mo6+ in the surface of MoO2/NC could be caused by its oxidation in air since monoclinic MoO2 is a metastable phase. Besides, one extra weak peak of Mo 3d located at 228.9 eV is correlated with the Mo–N bond. In the case of binary MoSe2/NC, the doublet peaks at the binding energies of 229.2 and 232.3 eV can be attributed to the Mo 3d5/2 and Mo 3d3/2 spin-orbits of Mo4+ in the environment of MoSe2. The oxidation of Mo4+ by air is not obvious for MoSe2/NC because there are no obvious peaks at higher binding energy. Moreover, there are no deconvoluted peaks characteristic of the Mo–N bond. Therefore, it is speculated that the presence of Mo6+ in the ternary MoSe2/MoO2/NC should originate from the oxidation of the MoO2 phase by air, while the Mo–N bond is most probably formed between MoO2 and nitrogen-doped carbon phases.
All the TEM, EDS, XRD, Raman, and XPS results demonstrate that the obtained ternary hybrid MoSe2/MoO2/NC is composed of MoSe2, MoO2, and nitrogen-doped carbon. To quantitatively analyze the content of each phase in the ternary hybrid MoSe2/MoO2/NC, elemental analysis and inductively coupled plasma optical emission spectroscopy were used. The mass percentages of all the elements are listed in Table S1.† Through calculation, the mass fraction of MoSe2, MoO2, and nitrogen-doped carbon in the hybrid is around 39.4, 26.2, and 34.4 wt%, respectively.
The Na-ion storage performance of the as-prepared ternary phases MoSe2/MoO2/NC was investigated using a sodium disk as the counter electrode and compared with that of binary phases MoSe2/NC and MoO2/NC. Cyclic voltammetry (CV) was employed to study the redox reaction behaviour of the electrode materials and the CV curves obtained at a scan rate of 0.1 mV s−1 are shown in Fig. 5a, S11 and S12.† In the case of ternary phases MoSe2/MoO2/NC, during the first negative scan, there are three reduction peaks at around 1.1, 0.6, and 0.2 V, which are similar to those of MoSe2-based electrodes reported in the literature.9,21,25,27 The first reduction peak at 1.1 V is usually considered to be the intercalation of Na-ions into the MoSe2 lattice accompanied by the formation of the NaxMoSe2 phase. The other two reduction peaks at 0.6 and 0.2 V correspond to the solid-state interphase (SEI) film formation via the reductive decomposition of electrolyte and the conversion reaction from NaxMoSe2 to Mo/Na2Se, respectively.44 The following positive scan corresponds to the desodiation process, during which the main oxidation peak at 1.8 V and the shoulder-like peak at 2.2 V are in good agreement with the reported oxidation peaks of MoSe2-based electrodes in SIBs.21,25 The reaction mechanisms of these oxidation peaks are still controversial. Some researchers claimed that the desodiation process should be accompanied by the reversible conversion from metallic Mo back to MoSe2.17,23,24 Also, there are some reports proposing that the desodiation process is related to the oxidation of Na2Se rather than metallic Mo since Se instead of MoSe2 is obviously formed after the desodiation process.9,25,26 Through systematically studying the ex situ Raman spectra of MoSe2-based electrodes at different charge/discharge potentials, Yang et al.9 directly prove that Se is formed at the end of the first charge. Therefore, it is proposed that the Na-ion storage mechanism of MoSe2 after the first cycle most probably involves the reversible conversion reaction from Se to Na2Se.
The CV curves of MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC electrodes in the second cycle are compared in Fig. 5b. The two couples of redox peaks at 1.7/2.1 V and 1.3/1.7 V observed for binary phases MoSe2/NC are typical of MoSe2-based electrodes in SIBs. Abouimrane et al.45 previously studied the Na-ion storage behaviour of a Se electrode and observed two discharge plateaus at 1.9 and 1.5 V in the sodiation process, so they proposed a multi-phase conversion reaction of Se, where intermediate phase polyselenides may be formed. The two reduction peaks of MoSe2/NC in the second cycle appear at similar potentials of 1.7 and 1.3 V, which actually should correspond to two potential plateaus in the discharge curves, further suggesting that the Na-ion storage mechanism of MoSe2 should be analogous to that of Se. So, intermediate phase polyselenides could also be formed during the cycling of MoSe2-based electrodes.42 The dissolution and shuttling of polyselenides may lead to a rapid capacity decline of MoSe2-based electrodes. In the case of binary phases MoO2/NC, no significant redox peaks are observed due to the poor Na-ion storage ability of MoO2. Through comparing the CV curves of MoSe2/MoO2/NC and MoSe2/NC, the main differences lie in that the first reduction peak of MoSe2/NC at 1.7 V is not clearly defined for MoSe2/MoO2/NC, but the reduction peak intensity of MoSe2/MoO2/NC at a lower potential of 1.3 V is much stronger. So it is assumed that such in situ formed ternary phases MoSe2/MoO2/NC could preclude the formation of intermediate phase polyselenides, which will be beneficial for the structural stabilization of electrodes during charge/discharge cycling.
Out of interest, the Li-ion storage behaviour of MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC is also investigated through CV (Fig. S13–S15†). In terms of MoO2/NC, the two couples of sharp redox peaks at 1.3/1.4 V and 1.6/1.7 V correspond to the phase conversion of MoO2 upon lithiation/delithiation.46 The CV curves of MoSe2/NC exhibit one couple of reversible redox peaks at 1.8/2.2 V, which are very similar to those of Se-based electrodes in Li–Se batteries.28,30,47 So the Li-ion storage mechanism of MoSe2 after the first cycle is acknowledged to be based on the reversible conversion reaction of Se to Li2Se.48 By analogy to the Li-ion storage of MoSe2, it is most likely that MoSe2 would exhibit a similar conversion reaction of Se to Na2Se. In the case of ternary phases MoSe2/MoO2/NC, the redox peaks of both MoO2 and MoSe2 are clearly identified, which is another piece of evidence proving the co-existence of MoSe2 and MoO2 in the hybrid.
The first three discharge/charge curves of the as-prepared hybrids at a current density of 0.14 A g−1 are shown in Fig. 5c. The reversible (charge) capacity of MoO2/NC is quite low (around 124 mA h g−1), and this is because the crystalline structure of MoO2 is not favorable for Na-ion storage. The discharge curves of MoSe2/NC exhibit a sloping potential plateau at around 1.5 V, corresponding to the two reduction peaks at around 1.7 and 1.3 V in CV curves. The reversible capacity of MoSe2/NC in the second cycle is around 413 mA h g−1, close to the theoretical capacity of MoSe2. By comparison with MoSe2/NC, MoSe2/MoO2/NC manifests a similar potential change tendency during discharge/charge, while its capacity is considerably enhanced. The reversible capacity of MoSe2/MoO2/NC at a current density of 0.14 A g−1 in the second cycle is around 634 mA h g−1, which is significantly higher than that of carbon nanosphere encapsulated MoSe2 (498 mA h g−1 at 0.1 A g−1),25 MoSe2-covered N, P-doped carbon nanosheets (454 mA h g−1 at 0.5 A g−1),9 and MoO2 nanocluster decorated MoSe2/graphene (422 mA h g−1 at 0.1 A g−1).42 To calculate the theoretical capacity of the ternary MoSe2/MoO2/NC phases, the theoretical capacity and mass fraction of each phase should be considered. The theoretical capacity of MoSe2 for Na-ion storage is 422 mA h g−1. However, it is difficult to determine the theoretical capacities of the other two phases MoO2 and NC because their crystalline structures are unfavorable for Na-ion storage and their Na-ion storage capacity should mainly be capacitive. So here the practical capacity of MoO2/NC (124 mA h g−1) is assumed as the theoretical capacity of the other two components (MoO2/NC). Taking the mass fractions of MoSe2 and MoO2/NC (39.4% and 60.6%, respectively) into consideration, the theoretical capacity of the ternary phases is calculated to be 241 mA h g−1. The considerably enhanced capacity of MoSe2/MoO2/NC as compared to the theoretical value suggests a strong synergistic effect of the ternary phases for Na-ion storage.49 Firstly, the numerous pores in MoSe2/MoO2/NC as observed from TEM images are capable of accommodating Na-ions. Especially, the PDA-derived N-doped porous carbon can provide more active sites for Na-ion storage than undoped carbon. Secondly, the unique structure of MoSe2/MoO2/NC with ultrasmall MoSe2/MoO2 nanocrystallites uniformly embedded in the carbon matrix not only increases the electroactive sites but also favours electronic transport, thereby giving rise to a high utilization efficiency of active materials. Thirdly, the polymer/gel-like film formed on the electrode surface could reversibly store/release Na-ions, which generates some extra capacity for the MoSe2/MoO2/NC electrode. Lastly, besides the Na-ions stored in the bulk phase of MoSe2, some Na-ions may be stored in the pores or interstices of the ternary phases MoSe2/MoO2/NC. Pak and Stucky et al.50 reported that nanoscale pore engineering of MoO2 enables the formation of a metallic Li-rich phase between the Li-ion intercalated MoO2 phase, so its practical Li-storage capacity is considerably higher than the theoretical value. Similarly, it is also very probable that a metallic Na-rich phase may be formed in pores or interstices during the sodiation of MoSe2/MoO2/NC. All these factors contribute to the high capacity of the ternary phases MoSe2/MoO2/NC.
The rate behaviour of the as-prepared hybrids was tested by discharging the electrodes at a current density of 0.14 A g−1 and charging them at various current rates ranging from 0.14 to 70 A g−1. As shown in Fig. 5d, the MoSe2/MoO2/NC electrode exhibits an average capacity of 611, 594, 534, and 461 mA h g−1 at current densities of 1.4, 7.0, 35, and 70 A g−1, respectively. Once the current density is returned to 0.14 A g−1, the capacity rapidly recovers to 640 mA h g−1. The maximum current density used for the rate behaviour evaluation of MoSe2-based electrodes in previous reports is usually up to 10 A g−1. The high capacity of MoSe2/MoO2/NC at extremely high current densities of 35 and 70 A g−1 suggests its excellent high-rate capability, which undoubtedly should be related to the unique structure of ternary phases. In the MoSe2/MoO2/NC hybrid, ultrasmall MoSe2 and MoO2 nanocrystallites are strongly embedded into or surrounded by carbon, which can offer omnibearing electronic transport pathways through the whole electrode. Compared to the MoSe2/carbon nanocomposites with carbon coated onto or encapsulated into MoSe2 active materials, where the carbon can not provide effective conductive pathways from the bottom or top, the supermolecule-derived embedding-type MoSe2/MoO2/carbon nanocomposites possess unique advantages in electron transport. The nitrogen-doping of carbon can further increase its electronic conductivity, benefit its affinity to electrolyte, and also increase its electroactive sites for Na-ion storage. Furthermore, in the ternary MoSe2/MoO2/NC nanocomposites, the presence of the Mo–N bond as revealed by the XPS results could lead to an enhanced interfacial interaction between MoSe2/MoO2 and N-doped carbon because some nitrogen may be simultaneously coordinated to Mo and C. As a result, an intimate contact between MoSe2/MoO2 and N-doped carbon is achieved, which will facilitate the transport of electrons and Na-ions across the interface of heterophases. The good electronic conductivity of MoO2 resulting from the existence of delocalized electrons in its conduction band also facilitates the electronic transport of the ternary MoSe2/MoO2/NC electrode.46,51–53 In addition, the porous structure of carbon and ultrasmall nanocrystallite size of MoSe2/MoO2 can facilitate the access of electrolyte to the active material and shorten the diffusion distance of Na-ions in the electrode bulk. As a result, not only the charge-transfer reactions on the electrode/electrolyte interfaces but also the diffusion of Na-ions in the solid phase will be favourable, which bring about the excellent rate behaviour of MoSe2/MoO2/NC. By contrast, the binary phases MoO2/NC exhibit extremely low capacity at high current rates due to the low Na-ion storage capability of MoO2. The reversible capacities of MoSe2/NC at various current rates are obviously lower than those of MoSe2/MoO2/NC, suggesting the synergistic effect of ternary phases for improving the Na-ion storage capacity and rate performance.
To gain insight into the electrode reaction dynamics of MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC, electrochemical impedance spectroscopy (EIS) was used. The Nyquist plots of the three electrodes after five complete sodiation/desodiation cycles are shown in Fig. 5e. The diameters of the depressed semicircles at medium-to-high frequency reflect the charge-transfer resistance (Rct) occurring on the electrode/electrolyte interface, while the inclined lines in the low frequency zone are ascribed to Warburg impedance, which is associated with solid-state Na-ion diffusion in the electrode bulk.44 The Rct value of MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC is 67, 154, and 627 Ω, respectively. As we know, the charge-transfer reaction dynamics of the electrode is related to the transport of both electrons and Na-ions. Even though MoO2 should have better electronic conductivity, its Na-ion transport ability should be very poor during the electrochemical reactions as reflected by its very low Na-ion storage capacity. The much lower Rct of MoSe2/NC as compared to that of MoO2/NC suggests that the Na-ion transport ability of the electrode is also of great importance for a decreased Rct. Therefore, a synergistic effect of MoSe2 and MoO2 gives rise to the lowest Rct of ternary MoSe2/MoO2/NC, suggesting a rapid charge transfer reaction on the electrode/electrolyte interface. As estimated from the slope of the inclined lines at low frequency, the Na-ion diffusion resistance in the MoO2/NC electrode should be significantly higher than that in the other two electrodes. The different rate behaviour of MoSe2/MoO2/NC, MoSe2/NC, and MoO2/NC can be perfectly explained by their different charge transfer and Na-ion diffusion resistances. Specifically, the lower the resistances are, the better the rate behaviour is.
The long-term cycling performance of the MoSe2/MoO2/NC electrode is shown in Fig. 5f. The reversible capacity of MoSe2/MoO2/NC discharged/charged at 2.1 A g−1 is stabilized at around 610 mA h g−1 after the initial several formation cycles, and manifests negligible degradation during the subsequent 1000 cycles. At a higher discharge/charge rate of 7 A g−1, the reversible capacity of the 1000th cycle is around 480 mA h g−1, equalling to a capacity retention of around 91%. The electrochemical performance of some previously reported MoSe2-based anodes for Na-ion batteries is summarized in Table S2.† For instance, MoSe2-covered N, P-doped carbon nanosheets exhibit an initial Na-ion storage capacity of 378 mA h g−1 and a capacity retention of 87% after 1000 cycles at 0.5 A g−1;9 encapsulation-type structured MoSe2@hollow carbon nanospheres preserve a capacity of 501 mA h g−1 after 1000 cycles at 1 A g−1.23 These comparative data suggest the outstanding cycling stability of MoSe2/MoO2/NC for Na-ion storage, which undoubtedly is related to its unique structure and ternary phase composition. The pores and voids in the hierarchical structured MoSe2/MoO2/NC hollow microspheres assembled from ultrathin nanosheets work as the buffering areas to alleviate the volume change of MoSe2 upon sodiation/desodiation, enabling the electrode structure to be stable. TEM images of the MoSe2/MoO2/NC electrode after 1000 cycles (Fig. 6) show that not only the hollow microspherical structure but also the overall dimensions of these microspheres are well maintained, validating the structural stability of MoSe2/MoO2/NC during repeated sodiation/desodiation reaction. Also, the embedding-type structure of the in situ formed ternary phases MoSe2/MoO2/NC renders a good contact among the three heterophases, and the surrounding MoO2 and NC phases can restrict the aggregation of MoSe2 active materials during long-term cycling. In addition, by analogy to the sulphur-based cathodes in Li–S batteries, where both porous MoO2 and nitrogen-doped carbon have been combined with sulphur to prevent polysulfide dissolution and improve the cycling performance,32,42 the presence of MoO2 and nitrogen-doped carbon in the ternary phases MoSe2/MoO2/NC is supposed to play the same role of trapping polyselenides generated by the sodiation/desodiation reaction of MoSe2. Correspondingly, the cycling performance of MoSe2/MoO2/NC for Na-ion storage is significantly improved through the rational construction of embedding-type structured ternary phases.
Footnote |
† Electronic supplementary information (ESI) available: Experimental section, Fig. S1–S15 and Tables S1 and S2. See DOI: 10.1039/c9na00815b |
This journal is © The Royal Society of Chemistry 2020 |