Petra Jarolimova*a,
Barbora Voltrovabc,
Veronika Blahnovabde,
Vera Sovkovabe,
Eva Pruchovaa,
Vojtech Hybaseka,
Jaroslav Fojta and
Eva Filovabd
aDepartment of Metals and Corrosion Engineering, Faculty of Chemical Technology, University of Chemistry and Technology, Technická 5, 166 28 Prague, Czech Republic. E-mail: jarolime@vscht.cz
bDepartment of Tissue Engineering, Institute of Experimental Medicine of the Czech Academy of Sciences, Vídeňská 1083, Prague 4, 142 20, Czech Republic
cFaculty of Science, Charles University in Prague, Albertov 2038/6, 128 00 Prague, Czech Republic
dSecond Faculty of Medicine, Charles University in Prague, V Úvalu 84, 150 06 Prague, Czech Republic
eUniversity Centre for Energy Efficient Buildings, Czech Technical University in Prague, Třinecká 1024, 273 43 Buštěhrad, Czech Republic
First published on 13th February 2020
Titanium and its alloys are widely used for substitution of hard tissues, especially in orthopaedic and dental surgery. Despite the benefit of the use of titanium for such applications, there are still questions which must be sorted out. Surface properties are crucial for cell adhesion, proliferation and differentiation. Mainly, micro/nanostructured surfaces positively influence osteogenic differentiation of human mesenchymal stem cells. Ti6Al4V is a biocompatible α + β alloy which is widely used in orthopaedics. The aim of this study was to investigate the interaction of the nanostructured and ground Ti6Al4V titanium alloys with simulated body fluid complemented by the defined precipitation of hydroxyapatite-like coating and to study the cytotoxicity and differentiation capacity of cells with such a modified titanium alloy. Nanostructures were fabricated using electrochemical oxidation. Human mesenchymal stem cells (hMSC) were used to evaluate cell adhesion, metabolic activity and proliferation on the specimens. The differentiation potential of the samples was investigated using PCR and specific staining of osteogenic markers collagen type I and osteocalcin. Our results demonstrate that both pure Ti6Al4V, nanostructured samples, and hydroxyapatite-like coating supported hMSC growth and metabolic activity. Nanostructured samples improved collagen type I synthesis after 14 days, while both nanostructured and hydroxyapatite-like coated samples enhanced collagen synthesis on day 21. Osteocalcin synthesis was the most enhanced by hydroxyapatite-like coating on the nanostructured surfaces. Our results indicate that hydroxyapatite-like coating is a useful tool guiding hMSC osteogenic differentiation.
Another strategy for improving osseointegration is the preparation of nanostructured surface on titanium alloys. Electrochemical oxidation in fluorides containing electrolytes leads to self-organised TiO2 nanotube layer formation on the surface. It is possible to easily control the diameter and length of the nanotubes by adjusting experimental conditions, such as the electrolyte composition, potential setting or temperature. Diameters of nanotubes ranging between 20–100 nm are the most common.9–12 Selecting the most appropriate nanotube diameter is very important especially for cell interaction. Nanotubes of smaller diameters (15–30 nm) are known to support cell adhesion, while nanotubes of larger diameters (80–100 nm) have been reported to support osteogenic differentiation but can also result in programmed cell death.13,14 So changed nanotopography of the material can improve cell adhesion which is crucial for an implants osseointegration.15 The process of osseointegration is driven by supporting the adsorption of proteins such as vitronectin or fibronectin, which mediate the signals between cells and material surface. It is well known that cell adhesion is not influenced only by surface properties, but also by material chemistry and charge distribution.16–18
As mentioned above, the binding of bone and metal implants is mediated by the formation of an apatite layer on the implants surface. Therefore, the presence and morphology of the apatite layer can dramatically influence cell adhesion, differentiation and finally implant integration. Hydroxyapatite coated titanium showed better osteoinductivity and osteoconductivity as compared to untreated titanium surfaces.19 For successful implant integration, biologically effective ions Ca and P are very important for cell adhesion, differentiation and growth of osteogenic cells, and contribute to bone resorption and osteoclastogenesis as well.20–23
Various techniques for the coating of titanium and its alloys with Ca–P layer have been studied, including the sol–gel method,24 the ion beam assisted vapour deposition method,25 the plasma spraying method,26 the electrochemical deposition method27 and phase-transited lysozyme coating.28 The exposition of titanium in a simulated body fluid (SBF) in order to create Ca and P-containing layer was also investigated. It was revealed, that the presence of the nanostructure enhances calcium and phosphate deposition and titanium surfaces can be spontaneously covered with hydroxyapatite-like layer via exposure to SBF.29
The purpose of the present work was to study the interaction of human mesenchymal stem cells (hMSC) with HAp-like coating on ground and nanostructured surfaces of the Ti6Al4V alloy. To investigate the biocompatibility effect of nanostructured samples with and without the HAp-like coating, in vitro cultivation using human mesenchymal stem cells (hMSC) was applied, whereas a glass coverslip was used as reference.
Ion | Concentration [mmol dm−3] | Ion | Concentration [mmol dm−3] |
---|---|---|---|
Na+ | 142.0 | HCO3− | 27.0 |
K+ | 5.0 | SO42− | 1.0 |
Ca2+ | 2.5 | Cl− | 109.0 |
Mg2+ | 1.5 | HPO42− | 1.0 |
After reaching 70% of confluence, the hMSC passage 4 were seeded on Ti6Al4V disc scaffolds and control glass coverslips at a density of 12000 cells per cm2. The cells were cultured in basic medium. After 3 days of cell culture when the cells reached confluence, cultivating media were enriched by osteogenic differentiation additives: 40 μg mL−1 ascorbate-2-phosphate, 100 nM dexamethasone, and 10 mM glycerol-2-phosphate disodium salt. The osteogenic medium was changed twice a week.
Fluorescence intensity was counted from 8 to 9 photomicrographs from each sample group using MATLAB. The intensity was normalized for the number of cells and related to the mean of the control glass.
Fig. 1 The nanostructured surface of Ti6Al4V alloy with cavities after beta phases (yellow arrows), SEM. Right image corresponds to the magnified marked square on the left. |
Fig. 2 The relative distribution of nanotube diameters created on Ti6Al4V by anodic oxidation at 30 V. Diameters were evaluated from 100 areas on 5 samples. |
Fig. 3 SEM image of ground specimen (a and b) and nanostructured specimen (c and d) after the exposure in SBF. |
In the case of specimen with nanostructured surfaces, the time dependency of open circuit potential and polarization resistance was different in comparison with the ground surface. Open circuit potential was decreasing to −10 mV after approximately 50 hours of exposure time. In contrast, the value of polarization resistance was increasing as in the case of ground sample (ESI Fig. S2†). Also, the impedance spectra of nanostructured surfaces (Fig. 5) are different as compared to the ground alloy. Their shape is influenced by the charge transfer through the nanostructured surface. The change in surface condition occurred after 18 hours, what was evident from impedance monitoring.
Fig. 5 Electrochemical impedance spectra of the specimen with nanostructured surface over exposure time. |
In this study, metabolic activity assay was employed to evaluate the viability of hMSC cultured on Ti6Al4V with four types of surfaces. 0 summarizes the absorbance of produced formazan by hMSC during 21 days of the culture. HMSC grown on all types of substrates, but significantly higher absorbance was measured on Ti and TiH when compared to both nanostructured samples N and NH on day 1. The highest values of metabolic activity were measured on glass on day 1 and 7. However, no significant differences in viability were observed among titanium samples on days 7–21.
The synthesis of collagen type I was evaluated from photomicrographs. As shows Fig. 9, nanostructures and HAp coating positively influenced collagen type I synthesis. On day 14, significantly higher fluorescence showed N and NH group compared to Ti and TiH. On day 21, higher collagen intensity was visible on both nanostructured samples and TiH than on Ti and glass. No significant difference was observed between N and NH on day 21.
The expression of osteogenesis-related genes and collagen synthesis were determined to assess the effect of surface modification on hMSC osteogenic differentiation. In parallel, 4 and 15 describe hMSC osteogenic differentiation trend cultured on four types of tested titanium surfaces and control glass coverslip for 21 days. It can be seen, that hMSC expressed COL1A2 similarly on all tested surfaces; the significant differences were visible only on day 14 in case of Ti and glass. Additionally, up-regulated expression of collagen at late stage of differentiation (day 21) were on glass compared to all titanium samples. However, partial detachment of cells from glass during medium exchange was observed and growing cells might have influenced this effect. No significant differences were observed in mRNA expression of late osteogenic markers osteocalcin (OCN) and integrin-binding sialoprotein (IBSP). The high increase of OCN and IBSP expressions were measured in all groups. On day 0, almost zero expression of IBPS was found (not shown) (Fig. 11).
The immunohistochemical staining of osteocalcin, a late marker of osteogenic differentiation, showed that the highest density of osteocalcin was present on nanostructured samples exposed to SBF and lower amount on ground samples exposed to SBF. Other samples showed only faint osteocalcin staining (Fig. 12).
In the first part of this study, the interaction of Ti6Al4V with simulated body fluid was investigated, when the two surface treatments were compared – ground and nanostructured surfaces. Many surface treatments of titanium alloys in order to enhance bioactivity and thus the cell differentiation and proliferation have been studied. Electrochemical oxidation under fixed experimental conditions in an electrolyte containing fluorides allowed the preparation of a well-defined and structurally arranged nanomorphology. Based on the previous study by Filova et al.,15 the oxidation process was managed at the potential of 30 V. In that investigation it was observed that nanotubes with the inner diameter of 50–80 nm obtained at the potential of 30 V had the best influence on bone cells adhesion, proliferation and differentiation. Also Oh et al. reported promoted MSC differentiation on nanotubes with diameter 70–100 nm thanks to stem cell elongation leading to cytoskeletal stress and enhanced differentiation into osteoblasts.31 Similarly, Lv et al. found that 70 nm was the optimal nanotube dimension for osteogenic differentiation of human adipose derived MSC in vitro and in vivo.
As mentioned above, Ti6Al4V is consists of α and β phases. The β phase is less corrosion stable than α phase because it is enriched with highly soluble vanadium compounds, thus β phase is etched preferentially. The area of the cavities covers approximately 11% of the whole surface as mentioned by Moravec et al.32
A wide range of electrochemical methods can be used to study the interaction of biomaterial with the human body environment. Open circuit potential for both ground and nanostructured specimens decreased until its stabilization at the value of −220 mV/ACLE in the case of ground surface and later at the value of −100 mV/ACLE for the nanostructured surface. Increasing polarization resistance values for both surface treatments could be explained by phase interface stabilization. The lower resistance value of the nanostructured surface is caused by the much larger surface of the nanotubes as compared to the ground surface.
Another method used was electrochemical impedance spectroscopy, which provides accurate and high-quality information on phase interfaces. The different shape of the impedance spectra is obvious when comparing the ground and nanostructured specimens. In the case of the ground sample, the spectrum from the first day corresponds to the passive layer and the other spectra already showed the change at the phase interface when the layer precipitated. The spectra obtained while exposing the nanostructured specimen have a totally different character; their shape is influenced by the charge transfer through the nanostructured surface.
Based on the measurement of impedance spectra over the entire frequency range, a 2 kHz frequency value was selected at which the greatest variances in phase angle and impedance module were detected. From the measurement of these parameters at a constant frequency of 2 kHz, it was possible to accurately evaluate the time of change on phase interface, hydroxyapatite (HAp) layer formation and growth was anticipated. This assumption was confirmed by EDS analyses after the exposure to SBF, when Ca and P were detected at an atomic ratio almost 1.67. The positive effect of the nanotubes is obvious from the single frequency results; the induction period of the nanostructured surface was about 12 hours shorter than that of the ground sample. Higher amount of Ca and P measured by EDS also confirmed the enhanced bioactivity of the nanostructured surface.
Also, the SEM microphotographs clearly demonstrated that formation of HAp-like layer was greatly enhanced by nanostructured surface. This outcome is in accordance with previous studies.29,33
From the biomedical point of view, the use of Ti6Al4V alloy for bone replacements could be occasionally viewed with apprehension, as elements Al and V are known for their possible cytotoxic effects.34–37 In earlier studies dealing with the form of these two elements in the nanotubes15,32 it was confirmed that Al is present in the form of Al2O3, also known as alumina, which is a widely used biomaterial that positively affects the adhesion and growth of osteoblasts,38 especially in the form of nanoparticles. In the case of V, this element was detected as oxide V2O5. Since the effects of V2O5 are more controversial.39,40
As a hydroxyapatite layer is more natural for cells than artificial surfaces, the surface covered by it may have improved biocompatibility and bioactivity. 3D-HAp/poly-d/l-lactide composites showed earlier osteoblast differentiation compared with β-TCP.41 In collagen composites with HAp, the osteogenic differentiation was influenced by concentrations of collagen, HAp, and pore diameter, with the best results on composite with 50 wt% Hap and 0.05% collagen.42 Similarly, Sun et al. reported better osteogenic differentiation of rat BMCs on collagen/HAp (60 wt% HAp) scaffolds than on β-tricalcium phosphate/Hap or pure HAp scaffold.43
Previous studies shown that micro- and nano-patterned HAp bioceramic surfaces enhance cell attachment and can stimulate osteogenic differentiation or bone regeneration.44,45 As an example, the micropatterned HAp surface showed strong osteoblasts contact guidance effect on 8 μm width microgrooves, whereas on larger patterns the cell alignment in the grooves direction proved to be weak.46 In another study, microgrooved HAp ceramic was applied to direct growth of osteoblasts.47
It was also shown that micro and nanostructures on bioceramic activate expression of different stem cell integrins. Zhao et al. described the synergic effect of hybrid micro/nanostructured surface of HAp bioceramics on osteogenesic differentiation of hBMSCs (human bone marrow stem cells). In addition, their results also revealed significantly enhanced cell adhesion, proliferation and expression of osteogenic genes on both patterned surfaces, compared to flat control.48
HAp coating with nanorod-structures on Ti6Al4V implants were applied to promote cell adhesion and osteointegration in diabetes mellitus rabbit models.49 The importance of distinct architecture of the biomaterial surface were recently reviewed. Cell fate is guided by the micro and nano patterned substrates, which influences protein adsorption, cell adhesion, migration, growth, differentiation and cell death. Various cell types differently react on the micro or nano patterned surfaces.50 In the study of Özçelik et al. BMSCs preferred smooth surface while osteosarcoma Saos-2 cells preferred nanopillar surfaces. However, the presence of fibronectin improved the BMSCs adhesion on nanopillar surfaces.51 The different behaviour of osteoblasts and myoblasts were strongly influenced by the width of HAp microgrooves prepared by photolithography, and subsequent coating with HAp.46
It is believed that nanotubes offer greater surface area for cell-biomaterial contact, and therefore better mimic bone architecture and function.13,14 Another approach to promote bone regeneration and new bone formation from the surrounding native bone is surface coating using SBF that create calcium phosphate structures similar to HAp of native bone.52,53 It was supposed that combining these two above mentioned surface modifications could greatly influence osteoinductivity and osteointegration of the Ti6Al4V implants.
For orthopaedic and dental implants success, not only osteoblast cells but also MSC play a key role in bone tissue regeneration. Recently, multipotent cells are becoming preferred model in a tissue engineering studies and hMSC are widely used as an osteogenesis model and for bone-tissue engineering applications. Therefore, in the current study hMSC were chosen to investigate the bioactivity of the created surfaces in vitro. NanoHAp coating of Ti specimen supported growth and osteogenic differentiation of hBMSC, which was enhanced by the addition of growth factors.54
From the previous studies it can be concluded that by specifically designing the nanotube diameter it is possible to support either hMSC adhesion or osteogenic differentiation.55,56 As was shown larger nanotube diameters lead to elongation of the cells and stimulate osteogenic differentiation via cytoskeletal stress.31 Moreover, it was clinically proven, that rough surfaces induce a more rapid osseointegration than the smooth surfaces57–60 and some of the porous Ti-based biomaterials are already in clinical trials.61
A crucial step for implant stability and subsequent cell differentiation is initial cell adhesion. This process is initiated by the adsorption of proteins from the body fluids to the implant surface that are recognised by the cell integrins, as the first step of the cascade leading to the formation of adhesion plaques. These highly organized protein complexes mediating ECM-cell contact but also act as mechanosensors that regulate cell phenotype.62 As was mentioned, focal adhesion complex consists of many proteins, where the mostly considered are talin, that forms a structural core of the focal adhesion, and vinculin which strengthens and stabilizes the focal adhesion complex.63,64
This phenomenon can be related to the fact that MSC were shown to adhere better on smaller nanotubes (30 nm), while larger nanotubes (100 nm) induced stem cell differentiation and proliferation.65 Although nanotubes with larger diameters were shown to be osteoinductive without the use of osteogenic supplements,13 other aspects such as cell sources, adsorbed proteins and their conformation, age and even the sex of the donor may influence cell response.66,67
In this study, cell attachment and morphology were evaluated 48 hours after seeding. Well spread polygonal-shaped cells were visible on all type of surfaces. Additionally, the distribution of molecular markers of cell adhesion, talin and vinculin, were evaluated by immunofluorescence staining. As shown in Fig. 7, vinculin was relatively diffused with well-developed focal adhesions on Ti and TiH group. Cytoplasmic talin was captured, but focal adhesions were not clearly visible.
Distribution of the vinculin positive areas in our work agreed with the study conducted by Saha et al. who showed dot-like cytoplasmic localisation of vinculin in osteoblasts on nanostructured Ti6Al4V68 and with our previous study using cpTi.69 We have shown similar dispersal of vinculin and talin in osteoblasts cultured one day on nanotubes with diameters among 24–66 nm.69
The study conducted by Filova presented the increase of both talin and vinculin concentrations in osteoblasts on nanotubes created by anodic oxidation at 30 V with an inside diameter around 35–80 nm compared to untreated Ti6Al4V.15 Costa et al. found that as roughness and complexity of HAp coated PCL matrices increased, the number of focal adhesions decreased.70
Higher vinculin staining implies that more focal adhesions were present in hMSC cultured on treated surfaces. The data suggest that increase in roughness could lead to enhanced initial adhesion. Similarly, increased formation of focal adhesions due to nano-roughened surface has been reported in osteogenic cells.71 We suggest that less developed focal adhesions on NH group could be caused by the phenomenon that nanotubes were overlapped by the HAp-like layer created by SBF treatment, therefore the simultaneous effect of nanotopography and HAp crystals could not be clearly detected. Our data indicating that talin synthesis or morphology were influenced by presence of the HAp. Talin intensity was lower on TiH and NH samples (Fig. 7) Colocalised F-actin and vinculin signal was visible only on Ti and TiH and glass group, but not on nanostructured groups which corresponds to our results on cpTi.69
A possible explanation of different results obtained from previous studies reporting focal adhesion formation,53,71,72 could be the shorter time of cultivation and possibly different type of integrins expressed in hMSC and other osteoblast cells.66 It has been shown that various types of integrins are expressed in osteoblasts.73 The type of expressed integrins subsequently determine important downregulated signalling pathways resulting in different cell fate and behaviour.62 Surface dependent expression of integrins described Brugge et al. in rat bone marrow cells cultured on titanium implants with various surface treatments.74 Other studies, considering substrate-dependent integrin expression, have shown that surface energy, chemistry and structure can fundamentally influence osteoblasts fate on titanium implants throughout integrin expression.75–78
In the present study, MTS assay was employed to evaluate the metabolic activity of hMSC cultured on different substrates. The method is based on the reduction of yellow MTS substrate by mitochondrial enzymes in living cells to water soluble purple formazan.
MSC grown on nanostructured surfaces NH and N displayed lower metabolic activity when compared to those cultured on Ti, TiH and glass on day 1. However, cell metabolic activity increased significantly in all samples and was similar on the titanium substrates from day 7 till day 21. It has been documented, that hMSC cultured on rough Ti surfaces decreased in cell number after 5 days of culture compared to smooth surfaces. The authors suggest that lack of proliferation was caused by the selection of hMSC compatible with growth on rough Ti surface or committed to osteogenic lineage, from phenotypically heterogenous hMSC population.79 Considering this, the observations of decreased cell numbers on TiH and N group are therefore no surprising.
To investigate the influence of modified titanium substrates on hMSC differentiation, osteoblast differentiation associated genes COL1A2, IBSP, and OCN were evaluated together with detection of selected proteins by immunohistochemical staining. Upregulated collagen type I synthesis was evident on both N and NH surfaces on day 14 and on all modified samples on day 21 (Fig. 10). Comparison of ground Ti and treated samples did not show any significant up-regulated expression of selected genes towards modified surfaces. However, the highest amount of mRNA for IBSP and collagen type I was found for TiH group, with the same trend in COL1A2 expression on day 14. High values of IBSP indicate the presence of terminal osteoblastic differentiation. IBSP, a non-collagenous osteogenic matrix protein, also known as marker of both terminal osteoblastic differentiation and new bone formation, is also believed to be involved in hydroxyapatite nucleation.80
On day 14, the exposition of Ti and N samples to SBF did not increase the collagen type I intensity on TiH and NH samples. Moreover, nanostructured samples showed significantly increased collagen intensity than other samples. However, on day 21, both nanostructured and HAp-modified samples showed a significant increase of collagen intensity compared to unmodified Ti and glass. Thus, the collagen formation is more influenced by nanostructured surface than HAp layer formation.
In our previous study, higher collagen synthesis on larger nanotubes (66 nm) compared to both smaller diameters and untreated surface were described.69 Current data correlate with upregulated collagen synthesis and no change in osteocalcin expression described previously on nanostructured implant surface in vivo, indicating an accelerated bone formation around the nanotubes.81
Furthermore, osteocalcin as an extracellular protein produced by differentiated osteoblast, indicating late stage of differentiation and mineralization stage.82 Although osteocalcin expression was not significantly affected by hereby used modifications, the numerous signals was visible on NH and less rare on TiH samples, compared to very rare signal on Ti but no signal on N and glass on day 21. The presence of osteocalcin (positive red signal in Fig. 12) suggests that MSC had differentiated into mature osteoblasts preferentially, mainly on HAp-like coated surfaces.
Oh et al. reported osteoblastic differentiation of human MSCs on nanotubes with higher diameter (70–100 nm) of nanotubes, but no osteogenic differentiation on nanotube with small diameter about 30 nm. Conversely, Park et al. reported better osteogenic differentiation of hMSC on 15 nm-diameter TiO2 nanotubes.83
The study conducted by Habibovic, showed positive effect of calcium phosphate coated Ti6Al4V on bone healing in vivo. Authors suggested that presence of calcium phosphate is important for ectopic bone formation.84 Also Barrere et al. reported enhanced bone integration in case of SBF mediated apatite-coated Ti6Al4V compared to noncoated implants on goat models.85 Cai et al. reported titanium (cpTi) treatment with potassium hydroxide and heat, and subsequent exposure to SBF and its effects on the rat BMSCs. The samples treated with potassium hydroxide, heat and exposed to SBF showed significantly higher metabolic activity, alkaline phosphatase activity and osteocalcin synthesis compared to pure cpTi. Samples treated with potassium and heat but not exposed to SBF did not show positive effect on BMSCs osteogenic differentiation.86
Considering above mentioned studies and our data, the SBF mediated mineralised surfaces of metal implants and other biomaterials have great future application, as this approach can be used for drug delivery that can dramatically enhance tissue regeneration. For instance, implant surfaces can be functionalised by the incorporation of bioactive molecules, such as antibiotics, growth factor and proteins, even nucleotide acids that can be used in gene therapy.52
In this study, we showed that nanostructured Ti6Al4V exposed to SBF was able to stimulate collagen type I and osteocalcin synthesis in hMSC, together with a high rate of cell growth.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/c9ra08912h |