Neeraj Sohal
,
Banibrata Maity
* and
Soumen Basu
*
School of Chemistry and Biochemistry, Thapar Institute of Engineering and Technology, Patiala 147004, India. E-mail: banibrata.maity@thapar.edu; soumen.basu@thapar.edu
First published on 23rd July 2021
Graphene quantum dots (GQDs) are carbon-based fluorescent nanomaterials having various applications due to attractive properties. But the low photoluminescence (PL) yield and monochromatic PL behavior of GQDs put limitations on their real-time applications. Therefore, heteroatom doping of GQDs is recognized as the best approach to modify the optical as well as electronic properties of GQDs by modifying their chemical composition and electronic structure. In this review, the new strategies for preparing the heteroatom (N, B, S, P) doped GQDs by using different precursors and methods are discussed in detail. The particle size, emission wavelength, PL emissive color, and quantum yield of recently developed heteroatom doped GQDs are reported in this article. The investigation of structure, crystalline nature, and composition of heteroatom doped GQDs by various characterization techniques such as high-resolution transmission electron microscopy (HRTEM), X-ray diffraction (XRD), Raman spectroscopy, Fourier transform infrared (FTIR) and X-ray photoelectron spectroscopy (XPS) are also described. The recent progress on the impact of mono or co-doping of heteroatoms on PL behavior, and optical, electrochemiluminescence (ECL), and electrochemical properties of GQDs is also surveyed. Further, heteroatom doped GQDs with attractive properties used in sensing of various metal ions, biomolecules, small organic molecules, etc. by using various techniques with different limits of detection are also summarized. This review provides progressive trends in the development of heteroatom doped GQDs and their various applications.
Since its discovery in 2008, GQDs are a new type of carbon-based fluorescent nanomaterial that have attained great attention in research areas due to their attractive properties.5 GQDs consist of highly crystalline graphene sheets having dimensions below 100 nm in one-, two- and few-layers (>10 layers).6 GQDs' structure has a thickness close to the dimensions of a single atom.7 Generally, GQDs contain sp2 or sp3 carbon atoms and functional groups based on oxygen. GQDs possess extraordinary properties, a size-dependent and non-zero electronic band gap as compared to bulk graphene. GQDs are designed when there is a fragmentation of graphene sheets into less than the exciton Bohr radius (20 nm).8 GQDs have exceptional properties such as PL, multi-color emission, brilliant photostability, biocompatibility, electrochemiluminescence (ECL), chemical inertness, small size derived from the quantum confinement effect (QCE), and edge effects. The carboxylic groups located at the edges of GQDs enhance their water solubility as well as providing the potential for functionalization with many inorganic, organic, polymeric, and biomolecules. These extraordinary properties of GQDs lead to enhancement of their applications in various fields such as energy storage,9 biosensing,10,11 bioimaging,12 drug delivery,13 photocatalysis,14 and many others. GQDs act as electron donors and acceptors owing to their great surface area and a huge number of edge sites. These properties increase the ECL and electrochemical activity of GQDs which further enhances their application in biosensing. In recent years, different mechanisms were reported for the PL emission of GQDs including QCE, recombination of localized electron–hole pairs, the zig–zag edge sites effect, the electronegativity of heteroatoms, and surface defects.15,16 GQDs can be synthesized by mainly two approaches i.e., the “top-down” approach and the “bottom-up” approach. In recent years, many researchers have synthesized GQDs by different methods under these two approaches.
The two contradictory PL emission behaviors i.e., excitation-independent and excitation-dependent found in GQDs and their exact mechanism are still under debate. Different luminescence colors can be attained by tuning the excitation wavelength or concentration of GQDs.16 By regulating size, shape, edge configuration, defects, functional groups, as well as heterogeneous hybridization of the carbon lattice, the PL emission of GQDs can be extensively changed from the deep ultraviolet region to the near-infrared region.17
In recent years, GQDs have been utilized as a great sensing platform for metal ions/biomolecules detection as compared to other standard methods. But the detection sensitivity decreases due to the poor quantum yield of GQDs. Therefore, surface functionalization and doping with heteroatoms such as nitrogen (N), sulfur (S), boron (B), and phosphorous (P) enhance the quantum yield of GQDs.18 Surface functionalization of GQDs through organic molecules and polymers occupies the specific functional positions on the GQDs which makes them selective for the sensing of metal ions and biomolecules. Heteroatom doped GQDs improve the physical as well as chemical properties such as chemical reactivity, optical activity, and electronic structure of GQDs by tuning their intrinsic properties.19,20 Hence, there is an urgent need to study the functionalized and heteroatom doped GQDs as they have great potential in biosensing.
There are different review articles available on the graphene quantum dots,4 heteroatom-doped carbon quantum dots,26 and heteroatom-doped graphene,27 but not specifically on the heteroatom-doped graphene quantum dots. Some reports discussed the general synthesis, properties, and application of GQDs. But in this article, we have discussed the synthesis of single and co-doped GQDs and their structural properties in detail. The detail investigation of different characterizations of heteroatom doped GQDs also reported here. Moreover, we have discussed the impact of heteroatom doping on the properties of GQDs and applications of heteroatom-doped GQDs as a sensor with their advantages and disadvantages. So, this review article will give all the detail information about the heteroatom-doped GQDs.
Fig. 1 Schematic representation of different methods to prepare N-GQDs by “top-down” approach: (a1) experimental set-up based on pulse laser ablation method, (a2) synthesis process by using GO and DETA,28 (b) nitrogen plasma treatment method performed in quartz chamber with 2.45 GHz microwave radiation,29 and (c) hydrothermal treatment of GO with ammonia solution.30 Part (a1) and (a2) are reproduced from ref. 28 with permission from [PCCP Owner Societies], copyright [2017], part (b) is reproduced from ref. 29 with permission from [American Chemical Society], copyright [2018], and part (c) is reproduced from ref. 30 with permission from [Royal Society of Chemistry], copyright [2013]. |
Recently, N-GQDs have been also prepared by using different carbon sources such as citric acid (CA), glucose, or glycine, and nitrogen sources such as ammonia, glycine, dicyandiamide (DCD), tris(hydroxymethyl) aminomethane, or 3,4-dihydroxy-L-phenylalanine, by using the hydrothermal method, microwave irradiations, or pyrolysis.24 These methods undergo main processes such as polymerization, carbonization, and further doping with nitrogen heteroatom in a single reaction for developing N-GQDs. Safardoust-Hojaghan et al.31 synthesized N-GQDs by using CA along with ethylenediamine under hydrothermal treatment. The hydrothermal treatment leads to the first carbonization of starting materials and then further converted into N-GQDs (Fig. 2a). The water-soluble N-GQDs have been developed through one-step high-temperature treatment. The CA (carbon precursor) and glycine (nitrogen precursor) undergo pyrolysis at 200 °C for the development of N-GQDs. The schematic illustration for the formation of N-GQDs is shown in Fig. 2b.25
Fig. 2 Schematic representation of one-step methods to prepare N-GQDs by “bottom-up” approach: (a) growth model from CA and ethylenediamine by using a hydrothermal method,31 (b) schematic illustration by high-temperature treatment,25 (c) digital image for the electrochemical set-up including o-phenylendiamine aqueous medium (left) and the product obtained after the completion of the reaction (right),32 (d) schematic diagram of the reaction mechanism of electropolymerization process32 and (e) synthesis process from glucose in ammonia solution by using microwave irradiations.24 Part (a) is reproduced from ref. 31 with permission from [Elsevier], copyright [2017], part (b) is reproduced from ref. 25 with permission from [Royal Society of Chemistry], copyright [2016], part (c) and (d) are reproduced from ref. 32 with permission from [Royal Society of Chemistry], copyright [2016] and part (e) is reproduced from ref. 24 with permission from [De Gruyter], copyright [2017]. |
Tian et al.32 prepared N-GQDs with large-scale –NH2 edge groups by using the “bottom-up” electrochemical method. They used only o-phenylenediamine (reactant) in an aqueous medium (electrolyte) and two highly pure platinum sheets as anode and cathode in this electrochemical method (Fig. 2c). They used dark conditions to remove the risk of spontaneous oxidation of o-phenylenediamine. Fig. 2d represents the formation mechanism of N-GQDs in which o-phenylenediamine is coupled together to form amine bonds. Further, the oxidative coupling occurs between partial amino groups and amine bonds which result in the development of phenazine structure. At the end of the reaction, there was the formation of N-GQDs with precise amino edge groups. There were several methods reported for the formation of N-GQDs but microwave irradiations provide fast and strong heating which completes the long hour reactions in few minutes. Zheng et al.24 used one-step microwave irradiations to develop N-GQDs in which glucose used as carbon precursor and ammonia as nitrogen precursor. They found that the ammonia used for the formation of N-GQDs was also acts as a catalyst for the dehydration reaction among molecules of glucose and water medium. Microwave heating enhances the reaction rate by providing rapid heat for glucose polymerization and carbonization and results in the fast formation of N-GQDs within 1 min. Fig. 2e represents the formation mechanism of N-GQDs. There were various one-step methods reported in the literature for the development of N-GQDs with variable sizes, PL emissive colors, and quantum yields are mentioned in Table 1.
Hetero-atom doped GQDs | Precursor | Synthesis & purification | Method | Size (nm) | λex (nm)/λem (nm) | QY (%) | Ref. & (year) |
---|---|---|---|---|---|---|---|
N-GQDs | GO + ammonia | The mixture of GO (dispersed in water) and ammonia was heated at 180 °C for 12 h using the hydrothermal method and then filtered | Hydrothermal treatment | 3.5 | 340/436 | 24.6 | 30 & (2012) |
The supernatant was dialyzed by a dialysis bag (3000 Da) for 2 h | |||||||
CA + hydrazine | (1) Pyrolyzing of CA by heating at 200 °C for 30 min | Multi-step hydrothermal treatment | 3.8 | 360/440 | 23.3 | 46 & (2014) | |
(2) Hydrothermal treatment of prepared solution at 180° for 12 h | |||||||
Centrifuge for 10 min | |||||||
CA + dicyandiamide | CA and dicyandiamide dissolved in water were heated at 180 °C for 3 h | Hydrothermal method | 2.3 | 370/452 | 36.5 | 47 & (2014) | |
The solution was centrifuged (12000 rpm) for 15 min and then dialysis membrane used (1000 Da) for 48 h | |||||||
CA + ammonia | Carbonization of CA with NH3 by heating at 200 °C for 3 h via hydrothermal method | Hydrothermal treatment | 3.5 | 325/420 | 30.7 | 19 & (2014) | |
A dialysis bag of 3000 Da was used for 4 h | |||||||
CA + glycine | The mixture of CA and glycine was heated at 200 °C for 5 min and an orange solution formed | High-temperature treatment | 1–4 | 355/450 | 28.1 | 25 & (2016) | |
No purification steps | |||||||
Glucose + ammonia | Glucose in distilled water with ammonia was heated at 900 W for 1 min through a commercial microwave oven | Microwave irradiation | 5.3 | 360/430 | 6.4 | 24 & (2016) | |
The solution was kept at 40 °C for 1 h and further, purified by dialysis membrane (1000 Da) | |||||||
o-Phenylene-diamine | o-Phenylenediamine was used as a reactant in water as an electrolyte. In this electrochemical process, 500 V was applied to the two Pt electrodes under dark conditions for 1 h | Electrochemical method | 3.9 | 420/569 | 71.0 | 32 & (2016) | |
No purification steps | |||||||
CA + ethylenediamine | The solution of equal ratio of CA and ethylenediamine was heated at 180 °C for 6 h | Hydrothermal treatment | 15–20 | 330/565 | 25.0 | 31 & (2017) | |
No purification steps | |||||||
Chitosan | Firstly, chitosan gets decomposed into N-compound and further HCN gets adsorbed on the copper's surface and then nucleation | Chemical vapor deposition (CVD) | 10–15 | 333/448 | — | 48 & (2018) | |
No purification steps | |||||||
C60/nitrogen plasma | The transformation of C60 molecules in a nitrogen plasma heated at 440 °C through microwave by using nickel foil as substrate | Plasma treatment by (CVD) technique | 4.5 | 336 to 392/412 & 432 | 7.4 | 29 & (2018) | |
No purification steps | |||||||
N-CNT/N-graphene in ammonia solution | N-CNT/N-graphene as the working electrode and the platinum sheet as counter electrode and ammonia solution as an electrolyte used in the two-electrode electrochemical system and 0.01 A charging current was supplied for 4–8 h | Electro-chemical method | 2.0 ± 0.5 | 380/455 | 19.3 | 49 & (2019) | |
Membrane filter with a pore size of 0.22 μm | |||||||
B-GQDs | Boron-doped graphene (BG) | First step, oxidation of BG to oxidized BG (BGO) by heating at 300 °C for 2 h in presence of HNO3 (40%) via tube furnace at inert atmosphere | Hydrothermal treatment | 2 to 4 | 310/440 | — | 50 & (2014) |
Second step, oxidation of BGO in presence of H2SO4 and HNO3 (1:3) for 17 h under ultrasonication. After adjusting the pH to 8, the solution was heated at 200 °C for 11.5 h | |||||||
The pale-yellow solution was filtered by a dialysis bag of 3500 Da for 12 h | |||||||
Graphite rod in 0.1 M borax | The voltage of 3 V was applied for 2 h at graphite rod (anode) dipped in 0.1 M borax and Pt sheet (cathode) undergo electrolysis | Electrolyzing method | 4.5 | 360/530 | 9.3 | 34 & (2016) | |
The prepared solution was filtered by 0.22 μM and then dialyzed with a dialysis bag (3500 Da) for 48 h | |||||||
Boron-doped graphene rods | B-doped graphene rods as anode and graphite rods as a cathode in the mixture of ethanol and water with 99.5:0.5 as electrolyte was used in an electrochemical process. The current intensity of 200–250 mA cm−2 for 2 h was applied for electrochemical reaction | Electrochemical method | 5 to 10 | 420/530 | — | 33 & (2016) | |
The resultant solution was centrifuged at 9000 rpm and purified by a dialysis bag of 1000 for 24 h | |||||||
VPBA (4-vinylphenylboronic acid) and boric acid | The sonication of VPBA and boric acid dispersed in acetone and ethanol for 30 min and further addition of H2O2. The solution was heated at 205 °C for 24 h | High-temperature treatment | 5.8 | 360/445 | 11.2 | 37 & (2016) | |
The prepared solution was centrifuged for 20 min at 20000 rpm for 3 cycles and dialyzed by dialysis bag (12000–14000 Da) for 3 days | |||||||
1,3,6-Trinitropyrene and borax in NaOH | Ultrasonication of 1,3,6-trinitropyrene and borax dissolved in NaOH solution for 30 min and heated at 200 °C for 6 h through hydrothermal treatment | Hydrothermal treatment | 2 | 480/520 | 16.8 | 35 & (2019) | |
The prepared solution was dialyzed by a dialysis bag (500 Da and 3500 Da) | |||||||
Boron carbide | Firstly, boron carbide converted to boron-doped graphene (BG) by heating at 1400 °C for 3 h | Microwave irradiation | 6 ± 2 | 320/420 and 440 | — | 38 & (2019) | |
Then, BG dispersed in polyethylene glycol heated at 220 °C for 30 min by microwave reactor | |||||||
The formed solution was dialyzed through a dialysis bag (14000 Da) for 2 days | |||||||
S-GQDs | Graphite in sodium p-toluenesulfonate aqueous solution | Graphite rod as working electrode dipped in sodium p-toluenesulfonate aqueous solution and Pt foil as the counter electrode was used in electrochemical process under voltage of 5 V for 3 h | Electrolyzing method | 3 | 380/480 | 10.6 | 43 & (2014) |
Filtered by 0.22 μM membrane and then, dialyzed by dialysis bag (3500 Da) for 1 day | |||||||
1,3,6-(Trinitropyrene + NaOH + Na2S) | The ultrasonication of 1,3,6-trinitropyrene dispersed in NaOH solution with Na2S for 1 h. Then, the solution was heated at 200 °C for 10 h | Hydrothermal treatment | 3 | 490/535 | 11.6 | 41 & (2016) | |
Filtered by 1000 Da dialysis bag for 2 days and then by 3500 Da for 1 day | |||||||
3-Mercaptopropionic acid (MPA) | Ultrasonication of a mixture of 1,3,6-trinitropyrene and MPA for 1 h. Further, the solution was heated at 200 °C for 10 h via hydrothermal method | Hydrothermal treatment | 2.5 | 360/450 | 9.2 | 42 & (2017) | |
Filter through 0.22 mm microporous membrane. Then, purified by dialysis bag of 3500 Da and 1000 Da for 24 h each | |||||||
CA + powdered S | CA and powdered S were dispersed in distilled water and then, heated at 170 °C for 4 h in an electric oven | Hydrothermal treatment | 3.93 | 380/460 | — | 44 & (2018) | |
The prepared solution was centrifuged (5000 rpm) for 5 min | |||||||
Green extract (sugarcane molasses) | Sugarcane molasses was stirred for 2 h and heated at 180 °C for 4 h | Hydrothermal treatment | 3.5 ± 1.25 | 380/515 | 47.0 | 45 & (2018) | |
The prepared black crude product was washed with water and filtered with many grade Gooch crucibles | |||||||
P-GQDs | Sodium phytate | The graphite rod as a working electrode and Pt electrode as a counter electrode used in an electrochemical process and sodium phytate solution as electrolyte. The voltage of 5 V was applied for 12 h | Electrochemical method | 2–4 | — | — | 39 & (2017) |
Filtered by 220 nm filter and purified by a dialysis bag (3500 Da) for six days |
Wang et al.37 used 4-vinylphenylboronic acid (VPBA) and boric acid under high-temperature treatment (200 °C) for the formation of B-GQDs. The two steps were involved in the formation of B-GQDs (Fig. 3a); the first step includes polymerization of VPBA molecules under high pressure and temperature and decomposition of H2O2 to form free radicals i.e., hydroxyl (HO˙) and hydroperoxyl (HOO˙) radicals. In the second step, the C–H bond in the benzene ring and O–B bond in boric acid were ruptured to produce B-doped carbon-based free radicals and further form bigger carbon-based fragments. The defects in the framework of GQDs enhance the active sites for the B-doping. Chen et al.34 synthesized B-GQDs by means of graphite rod in borax aqueous solution through the electrolyzing method. Ge et al.35 used a one-step hydrothermal method under the “bottom-up” strategy for the synthesis of B-GQDs through molecular fusion of 1,3,6-trinitropyrene and borax in NaOH solution. Vijaya et al.38 prepared B-GQDs by first converting bulk boron carbide (B4C) crystals into B-doped graphene (BG) followed by the uniform cutting of BG by using a microwave reactor. Tam et al.36 used a facile one-step hydrothermal approach at low temperature for the synthesis of B-GQDs by using glucose and boric acid. They prepared different types of B-GQDs with the variation in the B content and found that highly doped B-GQDs (up to 4.25%) showed exceptional electrocatalytic properties. They found an efficient method for preparing highly doped B-GQDs by using controlling the concentration of B. Zhang et al.33 used the electrochemical method for the formation of B-GQDs from a mixture of heteroatom salt in electrolyte and graphite rods as both cathode and anode. They prepared B-GQDs by electrolytic exfoliation of B-doped graphene rods which increase the uniformity of the B-GQDs.
Fig. 3 (a) stepwise formation mechanism of B-GQDs,37 (b) schematic diagram representing the synthesis of P-GQDs and its yellow emission under UV light (365 nm),39 and (c) schematic diagram showing the synthesis process of S-GQDs using bio-waste.42 Part (a) is reproduced from ref. 37 with permission from [Wiley Online Library], copyright [2017], part (b) is reproduced from ref. 39 with permission from [Royal Society of Chemistry], copyright [2017], and part (c) is reproduced from ref. 42 with permission from [Elsevier], copyright [2017]. |
Among different heteroatoms, S doping is distinct due to differences in the outmost orbitals of S and C makes an on-uniform spin density distribution that results in providing S-doped materials that show exceptional properties.41 S-atom is larger as compared to a carbon atom and the bond length of the C–S bond is 1.78 Å which is 25% greater in length as compared to the C–C bond. The electronegativity difference among S (2.58) and C (2.55) is very less which results in insignificant polarization or transfer of charge in the C–S bond. Therefore, S-doping into the structure of GQDs is quite hard due to difficulty in the formation of the C–S bond.41,42 Li et al.43 used an electrochemical method for the synthesis of S-GQDs through the electrolysis process of graphite present in sodium p-toluene sulfonate aqueous medium. Mostly, the hydrothermal treatment has been utilized for the development of S-GQDs as compared to the other methods. Bian et al.41 used a one-step hydrothermal reaction for the formation of S-GQDs based on aqueous-phase molecular fusion by using 1,3,6-trinitropyrene, Na2S, and NaOH. Bian et al.42 utilized 6-trinitropyrene as a carbon precursor and 3-mercaptopropionic acid (MPA) as a sulfur precursor for the development of S-GQDs through a hydrothermal approach (Fig. 3c). They found that the prepared S-GQDs have one layer graphene structure, uniformity, and exhibit strong blue emission. Jin et al.44 developed a simple one-step hydrothermal approach for preparing S-GQDs by using CA and powdered sulfur. They found that the prepared S-GQDs showed strong blue emission and have good water solubility as compared to undoped GQDs. Sangam et al.45 reported a hydrothermal approach for developing S-GQDs by using one precursor i.e., second generation green agro-industrial wastes. They developed a fast and eco-friendly method for the preparation of S-GQDs in which there was no requirement of catalysts or organic solvents.
Fig. 4 (a) Schematic diagram for the synthesis of free N, S-GQDs, and solidified GQDs,22 (b) preparation of B, N-GQDs by one-pot hydrothermal method,54 and (c) schematic diagram of developing N, S-GQDs with tunable luminescence.57 Part (a) is reproduced from ref. 22 with permission from [Elsevier], copyright [2017], part (b) is reproduced from ref. 54 with permission from [Elsevier], copyright [2020], and part (c) is reproduced from ref. 57 with permission from [Royal Society of Chemistry], copyright [2016]. |
The chemical doping of N as electron doping or B as hole doping into the structure of GQDs is easy due to quite similar atomic size. The electronegativity difference between C (2.55) and N (3.04)/B (2.04) is sufficient for the charge transfer in the C–N/C–B bond.34 Liu et al.51 described a rapid and facile process for the synthesis of B, N doped GQDs in which there was no requirement of any strong acid and surface deactivator. They prepared B, N-GQDs through pyrolysis in which CA, urea, and boric acid were used as precursors. Liu et al.54 used a “top-down” strategy for the synthesis of B, N-GQDs. They used GO, boric acid, and ammonia solution as precursors for the preparation of B, N-GQDs via a hydrothermal method (Fig. 4b).
The growth of co-doped GQDs with electron-rich N atom has forced to prepare the other new co-doped GQDs with electron-rich atoms, like P and S. Both P and S atoms have greater atomic radii as compared to carbon atoms and also the difference in the electronegativity of P (2.19), S (2.58), and C (2.55) is very less which result as insignificant charge transfer in C/P and C/S. Co-doping of GQDs into its structure with these elements was a quite difficult process and therefore, co-doped GQDs were exceptionally reported.55 Peng et al.56 described an electrochemical technique in which graphite electrode (C source), sodium phytate (P source), and sodium sulfide (Na2S) (S source) were used for the formation of S, P-GQDs. It was reported that the PL quantum yield of S, P-GQDs was greater than mono-doped GQDs i.e., S-GQDs and P-GQDs.55 Anh et al.18 reported a one-step hydrothermal approach for preparing N, S co-doped GQDs by using CA and thiourea. They found a high quantum yield of prepared GQDs in comparison with undoped GQDs. Xu et al.57 prepared two types of N, S co-doped GQDs by using polythiophene derived carbon source at different two temperatures. They found that two types of prepared GQDs showed different fluorescence and different properties due to variation in particle size as well as different surface defects. Fig. 4c represents the schematic presentation of the synthesis of N, S co-doped GQDs with different luminescence. Liu et al.58 formed N, P co-doped GQDs by using tetrakis(hydroxymethyl) phosphonium chloride (THPC) as carbon as well as phosphorous source and ethylenediamine endcapped polyethylenimine (PEI-EC) as nitrogen source and also passivation agent through hydrothermal treatment. Kundu et al.59 synthesized S, N, F co-doped GQDs by using multiwalled CNTs (MWCNTs) in ionic liquid i.e. 1-methyl-1-propylpiperidinium bis (trifluoromethylsulfonyl)imide through microwave treatment. They reported that microwave heating enhances the rate of the reaction with a high yield as compared to other conventional methods by the reduction of GO. The ionic liquid with exceptional chemical structure provides the efficient co-doping by N, S, and F heteroatoms. They also reported that, MWCNTs act as carbon source and the ionic liquid act as a strong source for N, S, and F in the preparation of N, S, F co-doped GQDs. Xu et al.52 developed N, P, S co-doped GQDs from anthracite coal (raw material) by using one-step wet chemical dialysis method. They reported an easy and cheap process for the preparation of N, P, S-GQDs. The different types of co-doped GQDs with synthesis methods, quantum yields, excitation and emission wavelength are tabulated in Table 2.
Co-doped GQDs | Precursor | Synthesis & purification | Method | Size (nm) | λex (nm)/λem (nm) | QY (%) | Ref. & (year) |
---|---|---|---|---|---|---|---|
N, F, S-GQDs | MWCNTs in a customized ionic liquid medium | MWCNTs dispersed in an ionic liquid by sonicating it for 1 h and then, kept for 15 min in a microwave (1100 W) | Microwave treatment | 2.0 | 375/409 and 435 | 70.0 | 59 & (2015) |
Filtered by 0.2 μm polytetrafluoroethylene (PTFE) membrane and dialyzed for 7–8 h | |||||||
N, S-GQDs | 1,3,6-Trinitropyrene + thiourea + DMF + NaOH | 1,3,6-Trinitropyrene and thiourea were dispersed in NaOH solution with DMF and sonicated for 30 min. The solution was heated at 200 °C for 10 h by using the hydrothermal method | Hydrothermal treatment | 2.1 | 375/450 | 23.2 | 53 & (2017) |
Filtered by a dialysis bag of 1000 Da for 1 day | |||||||
N, S-GQDs | CA + thiourea | CA and thiourea were dispersed in distilled water and then heated at 160 °C for 4 h | Hydrothermal treatment | 3.5 ± 0.5 | 340/445 | 41.9 | 18 & (2017) |
Centrifuged at 5000 rpm for 5 min | |||||||
B, N-GQDs | p-Phenylenediamine + formylphenylboronic acid | p-Phenylenediamine and formylphenylboronic acid were dispersed in ethanol and the solution was heated hydrothermally at 180 °C for 24 h | Solvent thermal method | 8.1 ± 1.2 | 400/560 | — | 60 & (2017) |
Filtered by 0.22 μm membrane and dialyzed for 48 h | |||||||
N, S-GQDs | CA + L-cysteine | The mixture of CA and L-cysteine in a round bottom flask was heated at 240 °C for 2 min and the orange color solution was obtained in 4 min | High temperature pyrolysis | 2.8 ± 1.0 | 350/430 | 84.0 | 61 & (2017) |
Filtered by a dialysis bag of 1000 Da for 8 h | |||||||
N, P, S-GQDs | Anthracite coal | Anthracite coal was dispersed in H2SO4 and HNO3 (3:1) and sonicated for 2 h. The mixture was heated in an oil bath for 1 day at 100 °C. The pH of the solution is adjusted to 7 | Wet chemical plus dialysis method | 1–7 | 420/515 | — | 52 & (2018) |
Filtered by 0.45 μm PTFE membrane and purified by dialysis bag of 500–1000 Da for 3 days | |||||||
S, P-GQDs | CA + sodium phytate + anhydrous sodium sulfate | The mixture of CA, sodium phytate, and Na2SO4 was heated at 180 °C for 7 h | Hydrothermal treatment | 3.5 | 340/440 | 15.6 | 55 & (2019) |
Centrifugation and dialysis of a prepared solution by using a dialysis bag (3500 Da) for 36 h | |||||||
P, S-GQDs | Graphite rod in a solution of sodium phytate, Na2S, and NaOH | Sodium phytate and Na2S were mixed in NaOH solution and used as electrolytes. The graphite rod as anode and Pt sheet as cathode dipped into prepared solution and voltage of 5 V was applied for 6 h | Electrolysis method | 3.2 | 440/530 | 39.5 | 56 & (2019) |
Filtered by 220 nm filter and dialyzed by a dialysis bag (3500 Da) for 48 h | |||||||
B, N-GQDs | GO, boric acid, and ammonia solution | GO was dispersed in distilled water and sonicated for 10 min. Then, the addition of ammonia and boric acid. The mixed solution was heated 180 °C for 20 h | Hydrothermal treatment | 3.8 | 322/422 | 5.1 | 54 & (2020) |
Filtered by 0.22 μm membrane and purified by a dialysis bag of 3000 Da for 2 days | |||||||
B, N-GQDs | CA + boric acid + urea | The mixture of CA, boric acid, and urea was heated for 2 h at 200 °C in an oven | Pyrolysis | 2.0 | 357/464 | 17.1 | 51 & (2020) |
Centrifuged (10000 rpm) many times and filtered by 0.22 μm microporous membrane. Further, dialyzed by using a dialysis bag (3000 Da) for 48 h |
We found from Tables 1 and 2 that different methods, precursors, and timing have been used for the synthesis of heteroatom doped GQDs. Table 3 represents the advantages and disadvantages of different methods used for the synthesis of heteroatom doped GQDs. Based on the information provided by Tables 1–3, we summarized all the methods based on their cost, efficiency, resources, timing, and safety. The synthesis based on microwave treatment was cheap, moderately efficient, very less time consuming, and safe. The synthesis based on the hydrothermal method was cost-effective, highly efficient, using economical resources, time-consuming, and safe. The wet chemical method based on acid treatment using coal was cheap, less efficient, a long-time process, but not safe. The electrochemical methods for the synthesis of heteroatom doped GQDs were highly efficient and safe, but expensive and time-consuming. According to the above literature, it was found that the hydrothermal method was most effective and mostly used for the synthesis of heteroatom doped GQDs.
Heteroatom doped GQDs | Method (precursors) | Advantages | Disadvantages | Ref. & (year) |
---|---|---|---|---|
N-GQDs | Hydrothermal (GO and ammonia) | - low cost | - Long synthesis process | 30 & (2012) |
- Potential for large scale production | ||||
- No strong acid treatment | ||||
Multi-step hydrothermal (CA + hydrazine) | - Cheap | - Highly toxic precursor (hydrazine) | 46 & (2014) | |
- Highly crystalline – uniform particle size | - Multi-step method | |||
Hydrothermal (CA + dicyandiamide) | - Excellent photostability | - Long purification time | 47 & (2014) | |
- Highly crystalline | - pH-sensitive | |||
- Good QY | ||||
- One-pot synthesis process | ||||
Hydrothermal (CA + ammonia) | - Facile | None | 19 & (2014) | |
- Low cost | ||||
- Less time for synthesis and purification | ||||
- One-step synthesis process | ||||
High temperature treatment (CA + glycine) | - Simple | - pH-dependent PL intensity | 25 & (2016) | |
- Inexpensive | ||||
- Only 5 min synthesis process | ||||
- Highly soluble in water | ||||
Microwave irradiation (glucose + ammonia) | - Simple | - Low QY | 24 & (2016) | |
- Only 1 min synthesis process | - Less doping of nitrogen content | |||
- Low cost | ||||
Electrochemical method (o-phenylene-diamine) | - High quantum yield | - Complex set-up | 32 & (2016) | |
- Large scale production | - Expensive | |||
Hydrothermal (CA + ethylenediamine) | - High stability | - Large particle size | 31 & (2017) | |
- Low cost | ||||
- Easy synthesis | ||||
Chemical vapor deposition (chitosan) | - Cheap precursor | - Complex process | 48 & (2018) | |
- No use of harmful acids | - Specific conditions | |||
- Single-step process | ||||
Chemical vapor deposition (C60/nitrogen plasma) | - One-step process | - Complex set-up | 29 & (2018) | |
- Uniform particle size | - Specific conditions | |||
Electrochemical (N-CNT/N-graphene in ammonia solution) | - Highly stable | - Specific membrane for purification | 49 & (2019) | |
- Highly crystalline structure | ||||
B-GQDs | Hydrothermal (boron-doped graphene) | - Homogenous and stable at room temperature | - Multi-step | 50 & (2014) |
- Uniform particle-size | - Strong acid treatment | |||
- Long synthesis process | ||||
- Long purification steps | ||||
Electrolyzing method (graphite rod in 0.1 M borax) | - Simple | - Specific purification conditions | 34 & (2016) | |
- Label-free | ||||
- Strong fluorescence | ||||
Electrochemical (boron-doped graphene rods) | - High stability | - Long synthesis process | 33 & (2016) | |
- Highly crystalline | ||||
- Good electrical activity | ||||
High-temperature treatment (VPBA and boric acid) | - Two-photon fluorescence | - Low quantum yield | 37 & (2016) | |
- NIR imaging | - Long purification process | |||
Hydrothermal (1,3,6-trinitropyrene and borax) | - Easy synthesis | - Particular purification steps | 35 & (2019) | |
- High yield | ||||
- Bright fluorescence | ||||
- One-step process | ||||
Microwave irradiation (boron carbide) | - High photoactivity | - Multi-step process | 38 & (2019) | |
- High temperature | ||||
- Long purification process | ||||
S-GQDs | Electrolyzing method (graphite in sodium p-toluene sulfonate aqueous solution) | - Good electrochemical reaction | - Filter membrane required | 43 & (2014) |
- Good surface chemical reactivity | ||||
- High photostability | ||||
Hydrothermal (1,3,6-trinitropyrene + NaOH + Na2S) | - High yield | - Low quantum yield | 41 & (2016) | |
- Stable fluorescence within a wide range of pH | - Two dialysis bags used for purification | |||
- High crystallinity | ||||
- Uniform size | ||||
Hydrothermal (MPA) | - One-pot synthesis | - Long purification process | 42 & (2017) | |
- Single-layer graphene structure | ||||
- Uniform size | ||||
Hydrothermal CA + powdered S | - Cheap and non-toxic precursor | None | 44 & (2018) | |
- Low-cost synthesis process | ||||
- High water solubility | ||||
Hydrothermal (sugarcane molasses) | - Green synthesis process | - Various grade Gooch crucibles are required for filtration | 45 & (2018) | |
- Good quantum yield | ||||
- Economical | ||||
- Facile | ||||
P-GQDs | Electrochemical (sodium phytate) | - Good electrochemical reaction | - Long purification process | 39 & (2017) |
- One-step synthesis process | ||||
N, F, S-GQDs | Microwave treatment (MWCNTs in a customized ionic liquid medium) | - One-step synthesis | - Specific conditions for filtration | 59 & (2015) |
- High quantum yield | ||||
- High yield | ||||
N, S-GQDs | Hydrothermal (1,3,6-trinitropyrene, thiourea, DMF, and NaOH) | - High yield | None | 53 & (2017) |
- Single-layer graphene structure | ||||
- Uniform size | ||||
- High crystallinity | ||||
N, S-GQDs | Hydrothermal (CA + thiourea) | - Good quantum yield | None | 18 & (2017) |
- One-pot synthesis | ||||
- Easy synthesis | ||||
- Cost effective | ||||
B, N-GQDs | Solvothermal (p-phenylenediamine + formylphenylboronic acid) | - Facile | - Specific conditions for purification | 60 & (2017) |
- One-pot synthesis method | ||||
- Cheap | ||||
N, S GQDs | High temperature pyrolysis (CA + L-cysteine) | - High quantum yield | - Long purification time | 61 & (2017) |
- Short synthesis process | ||||
- High ECL efficiency | ||||
N, P, S-GQDs | Wet chemical plus dialysis method (anthracite coal) | - Cheap precursor | - Strong acid treatment | 52 & (2018) |
- Facile oxidation process | - Harsh conditions for synthesis | |||
- Long process for purification | ||||
S, P-GQDs | Hydrothermal (CA, sodium phytate, and anhydrous sodium sulfate) | - High S and P doping | - Long purification time | 55 & (2019) |
- High water solubility | ||||
- Good stability | ||||
- Facile synthesis | ||||
P, S-GQDs | Electrolysis method (graphite rod in a solution of sodium phytate, Na2S, and NaOH) | - One-step electrolysis | - Long purification time | 56 & (2019) |
- Good electrolysis reaction | - Complex set-up | |||
B, N-GQDs | Hydrothermal (GO, boric acid, and ammonia solution) | - One-pot synthesis | - Low quantum yield | 54 & (2020) |
- Simple | ||||
- Cost-effective | ||||
B, N-GQDs | Pyrolysis (CA, boric acid, and urea) | - Easy synthesis | - Specific conditions and long purification process | 51 & (2020) |
- Cheap | ||||
- High crystalline |
Fig. 5 (a) TEM image and its HRTEM image (inset) of undoped GQDs,13 TEM and HRTEM images with particle size distribution histogram and lattice spacing of B-GQDs (b),35 N-GQDs (c),62 S-GQDs (d),44 P-GQDs (e),39 B, N-GQDs (f),54 and N, S-GQDs (g),18 respectively. Part (a), (b), (c), and (d) are reproduced from ref. 13, ref. 35, ref. 62, and ref. 44 with permission from [Elsevier], copyright [2018], [2019], [2020], and [2018], respectively. Part (e) is reproduced from ref. 39 with permission from [PCCP Owner Societies], copyright [2017], parts (f) and (g) are reproduced from ref. 54 and ref. 18 with permission from [Elsevier], copyright [2020] and [2017], respectively. |
Raman spectroscopy is used to examine the degree of disorder in the structure of the carbon matrix based on the different kinds of defects, for example, grain boundaries, point defects, stress, strain, stacking faults, edges, doping, vacancies, functional groups, and many others.45 The Raman spectra of GQDs and heteroatom doped GQDs consist of two bands were observed i.e., G band and D band. G band represents the E2g vibration modes of the aromatic sp2 carbon domains and the G band corresponds to the defects and structural disorder of sp2 domains.38 Mostly, the intensity fraction of D to G band (ID/IG) is utilized to investigate the order of structure among crystalline and amorphous systems of the graphitic domain. The values of ID/IG depend upon the type of method used for the synthesis of GQDs. A high value of ID/IG of heteroatom doped GQDs showed many defects on the surface of GQDs. Wang et al.17 determined the ID/IG value for GQDs, N-GQDs, S-GQDs, P-GQDs, and B-GQDs which were 1.01, 0.88, 0.86, 0.98, and 1.21, respectively (Fig. 6a). The number of defects follows the order such as B-GQDs > GQDs > P-GQDs > N-GQDs > S-GQDs.
Fig. 6 Raman spectra (a), XRD patterns (b), XPS spectra (c), and PL emission spectra excited at 360 nm (d) of GQDs, N-GQDs, S-GQDs, P-GQDs, and B-GQDs, respectively.17 Part (a), (b), (c), and (d) are reproduced from ref. 17 with permission from [Royal Society of Chemistry], copyright [2016]. |
Mostly, X-ray diffraction (XRD) patterns of undoped and heteroatom doped GQDs show a broad peak corresponds to the (002) graphitic lattice plane. The broad peak in the XRD pattern is due to the reduced size of the quantum dots. The small size of GQDs is responsible for its broad peak in the XRD pattern.63 The crystalline or amorphous nature of GQDs was investigated by the XRD pattern. Doping of heteroatoms such as boron having a greater size and less electronegativity than carbon can increase the interlayer spacing. In B-doped GQDs, the peak gets shifted towards the lower angle due to the participation of the boron atom in its graphitic structure which results in enlarging the interlayer spacing.8 In the case of N-doped GQDs, no increase in interlayer spacing was shown due to the less atomic radius of a nitrogen atom (65 pm) as compared to a carbon atom (70 pm). But the electronic structure gets altered due to the lone pair of the nitrogen atom. Therefore, in the case of N-GQDs, the peak shift to a higher angle corresponds to π–π stacking of graphene along with structural disorder due to doping of nitrogen. Fig. 6b shows the XRD pattern of GQDs, N-GQDs, S-GQDs, P-GQDs, and B-GQDs in which graphitic peak (002) was located at 22.77, 25.91, 25.03, 24.28 and 25.85°, representing interlayer spacing of 0.391, 0.344, 0.356, 0.367 and 0.345 nm, respectively. It was reported that, the interlayer spacing of undoped GQDs is greater as compared to graphite (0.334 nm) due to the existence of oxygen-containing groups.
The presence of chemical groups and heteroatom (N/S/P/B) as dopants slightly increases the interlayer spacing from graphite. But the large compacted interlayer spacing in heteroatom doped GQDs may be due to pyrolysis at high temperature.17 The functional groups (such as hydroxyl, carbonyl, epoxy/ether, and carboxylic acid groups) and elemental composition of heteroatom doped GQDs are determined by Fourier transform infrared (FTIR) and X-ray photoelectron spectroscopy (XPS) spectra, respectively.64 The electrochemical and optical properties depend upon the synthesis methods, heteroatoms, functional groups, and surface defects. Wang et al.17 determined the XPS measurements of undoped GQDs and heteroatom doped GQDs in which a major peak of graphitic carbon C 1s at 284.0 eV and O 1s at 531.2 eV was found. Other than C 1s and O 1s, the N 1s at 399.1 eV, S 2p at 164.3, P 2p at 133.8 eV, and B 1s at 192.4 eV have appeared in the XPS spectra of N-doped GQDs, S-doped GQDs, P-doped GQDs, and B-doped GQDs, respectively (Fig. 6c). XPS spectra confirmed the doping of heteroatom N/S/P/B into the framework of GQDs. They determined that the atomic ratio of different heteroatoms i.e., N, S, P, and B with respect to C was 17.36%, 1.60%, 1.78%, and 40.8%, respectively. Due to higher atomic radius of S12 and P, the atomic ratio of S and P was lower than N-GQDs and B-GQDs. Also, the intensity of O 1s increases due to doping of B as well P by bond formation with O and elimination of O by heat treatment cannot be achieved.
Fig. 7 PL spectra (a) and quantum yields (b) of heteroatom doped GQDs i.e., GQDs, S-GQDs, N-GQDs, and also S, N-GQDs.70 Part (a) and (b) are reproduced from ref. 70 with permission from [Elsevier], copyright [2019]. |
Feng et al.66 determined the effect of four heteroatoms including B, N, P, and S along with 3 different patterns on GQDs through time-dependent density functional theory (TD-DFT). They investigated the UV-visible spectra and HOMO–LUMO gaps for determining the relationships among the optical properties and doping of heteroatom on GQDs. They found that the heteroatoms make the formation of hybridization and therefore, a greater orbital hybridization leads to a high decrease in the HOMO–LUMO gap. In a comparison study, they found that the absorption spectra of N and S doped GQDs showed a minor hypsochromic shift, while B and P doped GQDs showed a blue shift for edge-doped GQDs in the pentatomic ring. Liu et al.58 observed the absorption spectra of N, P-GQDs in which dual absorption peaks located at 275 nm and 350 nm corresponds to π–π* transitions of aromatic π-domain in the carbon core and the absorption peak at 350 nm corresponds to n–π* transition of CO, CP, and CN bonds, respectively.
The GQDs consist of different surface functional groups and sp2 & sp3 carbon atoms which induce the surface state defects. The PL intensity decreases or increases with the variation of pH due to protonation and deprotonation. The reduction or oxidation of functional groups like –COOH and –OH present on the surface of GQDs put an impact on the PL intensity.72 This confirm that the optical properties of the GQDs are dependent upon the surface functional groups. The chemical modification of GQDs with different functional groups results in surface defects and put an impact on the PL intensity.76 Rajender et al.77 proved the PL emission of GQDs depends upon the surface defects by measuring the PL intensity in various solvents with different dielectric constants. They found that, the shift in the PL emission of GQDs present in different solvents was due to surface defects. The surface passivation with organic reagents has some drawbacks, like cytotoxic whereas doping with metal atoms results in non-uniform doping due to larger size than C atoms. Doping with non-metal atoms such N, S, P, B also induces the surface defects with uniform doping and enhances the fluorescence quantum yield of GQDs.78 Feng et al.66 found that the heteroatom doping assists charge transfer to occur in the excited state and diminish the electron and hole separation in the graphene structure. They found that, the big atoms incorporated on the basal plane show a crucial part in the recombination of electron density distribution in heteroatom doped GQDs by altering the geometry configuration. Also, the large atoms enlarge the HOMO–LUMO gap by transforming the sp2 hybridized carbon atom to sp3 hybridized. Various studies have been reported for the N-GQDs in which fluorescence is enhanced by doping of N atoms. The N atoms doped on the GQDs act as electron-rich active sites and enhance the radiative recombination and decrease non-radiative recombination.18 Also the sensing activity of N-GQDs depends upon the coordination performance of graphitic N atoms.32 Wang et al.17 observed that the emission wavelengths of GQDs (513.8 nm), N-GQDs (443.6 nm), P-GQDs (526.8 nm), and B-GQDs (525.2 nm) excited at 360 nm (Fig. 6d). In comparison with GQDs, N-GQDs and S-GQDs show a blue shift in the emission wavelength whereas P-GQDs and B-GQDs display a red shift in emission wavelength. They found that the emission wavelength follows the order i.e., B-GQDs > P-GQDs > GQDs > S-GQDs > N-GQDs.
In the case of some heteroatom doped GQDs, the synergistic effect of both QCE and surface defects leads to the origin of PL. Wang et al.55 prepared S, P-GQDs with large ratios of heteroatom doping i.e., S (9.66 at%) and P (3.34 at%). They found that the S, P-GQDs show high quantum yield as compared to monoatomic doped GQDs. The electronegativity variance among P (2.19) and S (2.58) result in the easy release of valence electrons of P as compared to S and also the high electron density of oxygen on GQDs enhances their synergistic effect. PL behavior of S, N-GQDs depends upon both the carbon core and surface functional groups.79
The PL mechanism is also based on the free zig–zag sites. Pan et al.80 prepared GQDs by hydrothermal cutting of GO and they obtained blue-emissive GQDs based on the free zig–zag sites effect. Radovic et al.81 revealed that zig–zag edges act like carbene sites (triplet state) and armchair sites act like carbyne sites (singlet state), both result in the origin of PL in GQDs. Lingam et al.82 studied the role of zig–zag edge sites in the origin of PL of GQDs with an experimental prove. They compared the PL results of GQDs, graphene nanoribbons (GNR), and carbon nano-onions (CNOs) and observed that the CNOs did not show any PL signal due to having a cage-like structure (no free edges). They found that, the free zig–zag edges present in GQDs are responsible for the PL emission. Yang et al.83 found that the free zig–zag sites of GQDs get protonated and showed less PL emission due to breakage of the emissive triplet state. On the other hand, the free zig–zag sites get restored in alkaline solution, result in PL recovery. Kumar et al.84 prepared amino-functionalized GQDs and found that the origin of PL emission depends upon the zig–zag effect. The PL of GQDs is also pH-dependent, such that on switching the pH between 1 and 12, the PL properties vary significantly. This process of varying pH is highly ascribed to the protonation and deprotonation of the free zig–zag or transmission sites of GQDs under alkaline and acidic conditions, thereby affecting the PL wavelength.85,86
The excitation-dependent and excitation-independent PL behavior of GQDs are still in debate. In the literature, different mechanisms were reported for both excitation-dependent and independent PL emission of GQDs. The excitation-dependent PL emission can be tuned by varying its excitation wavelength only and no need to modulate the structure of GQDs. Thus, this can be useful in various applications. The deviation in the energy band gap due to the size distribution of GQDs, result in excitation-dependent PL emission correlated with the QCE. But, excitation-independent PL emission was found in the case of large size distributions of GQDs. This proves that, size is not only the factor for the excitation-dependent PL emission.87 Among the different sizes, shapes, or surfaces of GQDs developed by different methods, some of them still have the same excitation-dependent PL properties.88 The excitation-dependent PL properties of GQDs are due to their different sizes, surface defects, QCE, conjugated sp2 π-domains, and zig–zag edge sites.88 Also, the functional groups present on the edges of GQDs introduce many excited states which result in radiative recombination of excited electrons and further lead to PL emission at different wavelengths.52 The surface defects also responsible for the excitation-dependent PL emission in GQDs. But there is no united agreement for surface state defects on the excitation-dependent PL emission due to having non-radiative traps.89 Heteroatom doping of GQDs also affects the size and surface functionalization of GQDs, which put an impact on its PL properties. Masteri-Farahani et al.90 found that the change in the size of S, N-GQDs leads to produce distinct sp2 clusters, and the electronic transitions from these sp2 domains resulted in PL emission shift. Also, the different functional groups present at the edges of S, N-GQDs lead to a generation of emissive traps between HOMO and LUMO levels due to which Stoke shift was observed along with excitation.
In the excitation-independent, the sample shows the same PL emission spectra at different excitation wavelengths. Wang et al.91 determined that S, N-GQDs showed excitation-independent PL and blue emission. They found that the excitation-independent PL was due to the uniform particle size of S, N-GQDs. Also, the doping of S eliminates the O-containing groups and increases the N-containing groups from the surface of GQDs via a cooperative effect that results in a new type of surface defect state. Zhu et al.92 observed that the GQDs showed excitation-independent PL behavior depends upon the surface states. They observed from the TEM images that, the particle size was not highly uniform. Thus, surface defects were more dominant for the excitation-independent PL emission as compared to the different particle sizes. Gu et al.93 prepared GQDs exhibiting excitation-independent PL emission due to more dominating surface state defects rather than size. The surface states consist sp2 carbon domain which is more uniform. Dong et al.94 observed excitation-independent PL emission of GQDs due to uniform distribution of both particle size and the surface defects consists of sp2 domains. Zheng et al.29 found that the N-GQDs were incorporated in the carbon framework having uniform size and result in excitation-independent PL emission.
Nanomaterials are acting as promising probes for environmental safety.116 The interactions among GQDs and specific substances can originate diverse effects in the fluorescent intensity of GQDs. Due to their intrinsic fluorescent properties, the intensity of GQDs either gets reduced or enhanced.117 Based on this principle, a variety of sensors have been developed for the determination of different metal ions, macromolecules (like DNA, RNA, proteins), small organic molecules, insecticides, and pesticides with good selectivity and sensitivity.108 Nowadays, GQDs-based sensors and biosensors are rapidly developed with stable PL, unique ECL, and electrochemical properties that are extremely sensitive for small perturbations.118 Therefore, GQDs-based sensors can be utilized for the selective detection of metal ions and biomolecules.119 The mechanism of these sensors is mostly based on the occurrence of charge transfer between the metal ion and GQDs due to shorter distance among them, thereby resulted in the quenched or enhanced PL. The functional groups present at the edge of GQDs enhance its water solubility as well as provides the potential for functionalization with many inorganic, organic, polymeric, and biomolecules. The ECL and electrochemical properties of GQDs are because of the electron-donating and accepting tendency of the GQDs owing to high surface area and large number of edge sites.86,118 These attractive properties of GQDs lead to enhance their application in biosensing.
In recent years, the GQDs-based sensors have been extensively used in the sensing probe for the efficient sensing of metal ions and biomolecules as compared to other standard methods. But the detection sensitivity decreases due to the poor quantum yield of GQDs. Therefore, to improve the performance of GQDs, they have been functionalized by surface modifications. And, this can be achieved by controllable oxidation degree, surface functionalization, and heteroatom doping with heteroatoms (N, S, P, and B) to enhance the quantum yield of GQDs.117 The doping and co-doping of GQDs generates additional coordination sites and provides more defects in the structure of prepared GQDs which eventually improves the physical and chemical properties, for example, chemical reactivity, optical properties, and electronic framework of GQDs by tuning their intrinsic properties.85,120 These heteroatom doped GQDs based biosensors have thus provided a new platform for early diagnosis of several diseases, improved biological agents, bioenvironmental monitoring, and safety assessment. Therefore, these GQDs become suitable probes for various sensing applications. The distinctive and recently designed GQDs-based biosensors are listed in Table 4.
Sensor | Materials | Detection target | Detection range | LOD | Advantages | Disadvantages | Ref. & (year) |
---|---|---|---|---|---|---|---|
PL sensor | Phosphorylated peptide–graphene quantum dot (GQD) | Protein kinase | 1.1–1.0 unit mL−1 | 0.03 unit mL−1 | - Simple | - Less sensitive | 136 & (2013) |
- Fast detection | |||||||
- Drug development | |||||||
B-GQDs | Glucose | 0.05–10 mM | 0.01 mM | - Label free sensing | - Sensitivity in mM range | 50 & (2014) | |
- High selectivity | - pH dependent detection | ||||||
GQDs@GSH | Cu2+ | 0.1–1.0 μM | 53 nM | - Act as dual probe | - Specific pH detection | 137 & (2015) | |
- Cell imaging | |||||||
- High sensitivity | |||||||
N-GQDs | Thia-cloprid | 0.1–10 mg L−1 | 0.03 mg L−1 | - Test strip-based sensor | - Long preparation process of test strip | 123 & (2018) | |
- High selectivity | |||||||
- Portable sensor | |||||||
GQD-polyacrylonitrile (PAN) membrane | Chlorine | 10–600 μM | 2 μM | - High reproducibility | None | 118 & (2018) | |
- No need of incubation time | |||||||
- High stability of sensor | |||||||
- Real sample detection | |||||||
S-GQDs-Al3 + (S-single layered) | Phosphate ion (PO43−) | 0.25–7.5 μM | 0.1 μM | - Label free | None | 138 & (2018) | |
- High selectivity | |||||||
- High reproducibility | |||||||
- Low cytotoxicity | |||||||
- Detection in water sample | |||||||
S, N-GQDs | Ascorbic acid | 10–500 μM | 1.2 μM | - Simple | - Less sensitive | 79 & (2019) | |
- Less time consuming | - No selectivity studies | ||||||
S, N-GQDs | Ag+ | 12–125 μM | 12.90 μM | - High selectivity | - pH dependent sensing | 119 & (2019) | |
Hg2+ | 12–125 μM | 9.14 μM | - Real sample detection | ||||
- Wide range of detection | |||||||
Maleimide-GQDs | Bithiol (GSH + Cys) | 5–400 nM | 1.69 nM | - Highly sensitive | - Long incubation time | 139 & (2020) | |
- Real sample detection | |||||||
- High reproducibility | |||||||
N-GQDs | Homo-cysteine | 5 × 10−11 to 5 × 10−8 M | 5 × 10−11 M | - Very low detection limit | None | 111 & (2020) | |
- PL sensing in living cells | |||||||
- Excellent selectivity | |||||||
N-GQDs | Hg2+ | 0.5–110 nM | 0.08 nM | - High sensitivity | None | 115 & (2020) | |
- Wide detection range | |||||||
- Real sample detection | |||||||
- Simple | |||||||
N-GQDs | Fe3+ | 0–200 μM | 0.87 μM | - Good selectivity | - Less sensitive | 135 & (2019) | |
- Easy | |||||||
- Simple | |||||||
- Low cytotoxicity | |||||||
ECL sensor | MoS2-GQDs | 2-Methyl-4-chlorophenoxyacetic acid | 10 pM to 0.1 μM | 5.5 pM | - Very sensitive | - Complex | 127 & (2017) |
- Real sample sensing | - Expensive | ||||||
- Good reproducibility | |||||||
Au@Ag/GQDs | HULC (highly up-regulated in liver cancer) | 1 fM to 5 nM | 0.3 fM | - Ultrahigh sensitive | - ECL response dependent on thickness of Au@Ag nanoparticles | 140 & (2018) | |
- Good selectivity | - Long time for fabrication | ||||||
- Good stability | - Complex | ||||||
AuNP-GQDs | Carcinoembryonic antigen | 0.1 pg mL−1 to 10 ng mL−1 | 3.78 fg mL−1 | - High sensitivity | - Specific pH detection | 141 & (2018) | |
- High reproducibility | - Long fabrication process | ||||||
- Good selectivity | |||||||
GQDs-AuNPs | Glucose | 0.1–5000 μM | 64 nM | - Sensing in complex human serum | -Temperature dependent | 125 & (2019) | |
- Good selectivity | |||||||
GQD/TiO2NTs | Prostate protein antigen | 1.0 fg mL−1 to 10 pg mL−1 | 1 fg mL−1 | - High stability | - Complex fabrication | 142 & (2019) | |
- Repeatable | |||||||
- Biological sample sensing | |||||||
NGQDs/boron nitride quantum dots | Folic acid | 1.0 × 10−11 M to 1.0 × 10−4 M | 5.13–10−12 M | - Very low detection limit | None | 124 & (2019) | |
- Good selectivity | |||||||
- High recovery | |||||||
- Simple | |||||||
-Real sample sensing | |||||||
AuNCs-GQDs | Pentoxifylline | 7.0 × 10−7 to 1.2 × 10−4 mol L−1 | 9.0 × 10−8 mol L−1 | - Good selectivity | None | 95 & (2019) | |
- Good reproducibility | |||||||
- Easy fabrication | |||||||
AuNP-GQDs-DNA S3 and DNA S2 | Hg2+ | 0.01 nM to 100 nM | 2.48 pM | - Ultrahigh selectivity | - Long incubation time | 143 & (2019) | |
- Excellent selectivity | |||||||
- Real sample sensing | |||||||
PICA/F–Au-GQDs [poly (indole-6-carboxylic acid)/flower–gold] | Aflatoxin B1 | 0.01–100 ng mL−1 | 0.00375 ng mL−1 | - Very detection limit | - Long fabrication process | 144 & (2020) | |
- Wide detection range | - Specific temperature detection | ||||||
- Real sample analysis | |||||||
Ru(pby)32+@N-GQDs | Ethosuximide (ESM) | 5.00 × 10−7 to 1.00 × 10−4 mol L−1 | 3.00 × 10−7 mol L−1 | - High selectivity | - Ratio dependent of composite | 126 & (2020) | |
- Real sample sensing | - Specific pH range for detection | ||||||
- Good recovery | |||||||
P, S-GQD | Okadaic acid (OA) | 0.01–20 ng mL−1 | 0.005 ng mL−1 | - Low detection limit | - Specific temperature and time for incubation | 56 & (2020) | |
- Low matrix effect | |||||||
- Advance fabrication | |||||||
N-GQDs | Quercetin | 2.0 × 10−9 to 1.6 × 10−6 M | 8.2 × 10−10 M | - Highly sensitive | - Complex | 145 & (2019) | |
- High accuracy | |||||||
- Wide detection range | |||||||
- High selectivity | |||||||
GQDs/GNPs/GCE | Luteolin | 1 × 10−8 to 1 × 10−5 M | 1.0 nM | - Low detection limit | None | 130 & (2019) | |
- Good selectivity | |||||||
- Real sample detection | |||||||
GQDs-MWCNTs | DA | 0.005–100.0 μM | 0.87 nM | - Excellent selectivity | None | 146 & (2020) | |
- Real sample detection | |||||||
- High sensitivity | |||||||
GQDs@MWCNTs/GCE | Dopamine (DA) | 0.25–250 μM | 95 nM and 110 nM | - High sensitivity | - Time consuming | 147 & (2020) | |
- Wide range of detection | |||||||
- Excellent electrocatalytic | - Expensive | ||||||
- Real sample analysis | |||||||
GC/GQDs-NF (NF-naflon) | Cd2+ | 20–200 μg L−1 | 11.30 μg L−1 | - Real sample detection | - Specific conditions | 120 & (2020) | |
- High accuracy | - Less sensitive | ||||||
GC/GQDs-NF | Pb2+ | 20–200 μg L−1 | 8.49 μg L−1 | - Real sample detection | - Specific conditions | 120 & (2020) | |
- High accuracy | - Less sensitive | ||||||
Au@Cu-MOF/N-GQDs | Patulin | 0.001–70.0 ng mL−1 | 0.0007 ng mL−1 | - Good selectivity | - Long fabrication process | 129 & (2020) | |
- Good accuracy | |||||||
- Very low detection limit | |||||||
MIP/GQDs-Pt nanoparticles | Sulfadimidine (SM2) | 0.1 nM to 0.1 mM | 0.023 nM | - Highly sensitive | - Particular conditions of fabrication | 134 & (2020) | |
- Computer simulation | |||||||
- Real sample analysis | |||||||
CdS/Au/GQDs | DA | 0.1 to 350 μM | 0.0078 μM | - Limit of detection lower than DA in biological tissues | - Complex process | 133 & (2020) | |
- Wide range of detection |
Fig. 8 (a) PL spectra and the inset image of test strip of N-GQDs/N-GQDs with thiacloprid under the UV lamp,123 (b) standard curve between PL intensity and concentration of thiacloprid,123 (c) PL responses of B doped GQDs with increase in the glucose concentration (1 to 200 mM) and inset image shows increase in PL under UV lamp with increase in the glucose concentration from left to right (0, 2, 8, 20, and 50 mM),50 and (d) standard plot between PL intensity and concentration of glucose in phosphate buffer of pH value of 7.4.50 Part (a), (b) are reproduced from ref. 123 with permission from [Elsevier], copyright [2018], and part (c), (d) are reproduced from ref. 50 with permission from [American Chemical Society], copyright [2014]. |
Zhang et al.50 have synthesized B-GQDs by using a hydrothermal approach for ultra-selective detection and sensing of glucose. The PL intensity of B-GQDs solution increases in the presence of different concentrations of glucose (1–200 mM) (Fig. 8c). Fig. 8d represents the plot of the PL intensity of B-GQDs with the different concentrations of glucose (1–200 mM) and the inset image reveals a linear curve for the determination of glucose (0.1–10 mM) with a limit of detection (LOD) value i.e., 0.03 mM. They observed the enhancement in the PL intensity of B-GQDs due to limitations on the intermolecular rotations started by unusual interactions of B-GQDs and glucose. This was due to the reaction between the dual cis-diol components present in glucose and dual boronic acid groups located on the surface of B-GQDs. Therefore, B-doping on the GQDs provides a novel type of surface state that gives rise to a new PL enhancement mechanism after the interaction with glucose.50
Zhang et al.126 fabricated Ru(pby)32+@N-GQDs [(tris(2,2′-bipyridyl)) ruthenium(II)@N doped GQDs] by electrostatic interaction between Ru(pby)32+ and N-GQDs, which showed excellent and stable ECL properties and acts as a PL sensing probe for the selective determination of ethosuximide (ESM) as shown in Fig. 9. The quantitative relationship among the different concentrations of ESM and variation in the ECL intensity was examined. This is used for reasonable detection in blank plasma and urine samples. Thus, such an efficient and simple MIP on Ru(pby)32+@N-GQDs system may be a good model for the fabrication of drug sensors and has a potential application to assay ESM in the biological samples. They found that the ECL intensity was reduced in the presence of different concentrations of ESM and ECL stability curve at each concentration (Fig. 10a). Fig. 10b shows a good linear relationship among ΔIECL (difference of the ECL intensity values in the presence and absence of ESM) and logarithm concentration of ESM with the detection range from 5.00 × 10−7 to 1.00 × 10−4 mol L−1 (Fig. 10b). Peng et al.56 synthesized water-soluble and uniform-size P, S-GQDs by electrolysis method and demonstrated advancement in ECL properties. The ECL immunosensor was designed for ultra-sensitive detection of okadaic acid (OA) using carboxylated multiwall carbon nanotubes–poly(diallyldimethylammonium) chloride–Au nanocluster (CMCNT-PDDA-AuNCs) composite as a sensing probe to immobilize OA and P, S-GQDs as effective ECL markers. The design of as prepared immunosensor showed high convenience, great sensitivity response, and minor matrix effect. These effective properties of prepared ECL immunosensor used for the OA sensing in mussel samples. Yang et al.127 fabricated molybdenum disulfide (MoS2) GQDs hybrid composite contributing excellent ECL performance. The MoS2-GQDs hybrid composite was fabricated as MIP-ECL sensor for the sensitive and selective detection of 2-methyl-4-chlorophenoxyacetic acid. The developed sensor showed great sensitivity, high selectivity, and stability for the detection of pesticides and veterinary drugs in food and environmental safety. Chen et al.128 synthesized a single luminophor dual-potential ECL system by using N-GQDs as a ratiometric sensor for the efficient detection of Co2+ ions. During the cyclic potential scanning, the dissolved oxygen changes to O2− and HO2− which get involved in the anodic and cathodic producing process of N-GQDs. Co2+ ion is used to play the catalytic activity in the intermediate steps of anodic ECL reactions to amplify the anodic intensity and decrease the cathodic ECL intensity due to inhibition and quenching effects on the excited state of the luminophor. The constructed ratiometric dual-potential ECL system shows excellent selectivity against other common metal ions. Utilizing the dual-potential ECL sensor makes the sensing more credible in principle. There have been various sensors developed based on ECL by using GQDs are reported in Table 4.
Fig. 9 The schematic diagram of MIP ECL sensor for the detection of ethosuximide.126 Image is reproduced from ref. 126 with the permission from [Elsevier], copyright [2020]. |
Fig. 10 (a) Relative ECL stability curve of MIP ECL sensor with the addition of different concentrations and (b) a calibration graph for the detection of ESM.126 Part (a) and (b) are reproduced from ref. 126 with permission from [Elsevier], copyright [2020]. |
Zhang et al.134 fabricated MIP/GQDs-Pt nanoparticles (PtNPs)/glassy carbon electrode (GCE) sensing system via a simple one-step electro-copolymerization method for highly sensitive detection of trace amount of sulfadimidine (SM2) in food. Using the dispersion-corrected (DFT-D) method, a comprehensive computer simulation strategy was used to combine molecular docking and the solvation effect in the screening of bi-functional monomers for the rational design of MIP materials. The sensor is better in terms of effective sensitivity, specificity, stability, ease of operation, and cost. The one-step electro-copolymerization process leads to a robust integration of MIP film with a transducer. Therefore, this method simplifies the preparation of MIP material and lowers the cost. The electro-copolymerization system also offers an important reference for the electro-polymerization reactions and may be extended to supercapacitors and fuel cells. Ibrahim et al.133 prepared a triple interconnected structure of cadmium sulfide (CdS) modified with Au/GQDs. The introduction of Au and GQDs on the photocatalytic active center of CdS acts as a charge separation mediator and photosensitizer, respectively, which are favorable for charge separation and transportation and PEC conversion. Fig. 11a showed the proposed mechanism of the CdS/Au/GQDs sensor in which CdS/Au/GQDs photoelectrode used for the detection of DA get oxidized to PDA which owns a large number of benzoquinone (BQ) groups (electron-acceptors). The photocurrent responses get reduced with the addition of DA (Fig. 11b). Fig. 11c showed a calibration curve for the sensing of DA with the detection ranging from 0.1 to 350 μM and the value for LOD was 0.0078 μM. Fu et al.135 synthesized N-GQDs, via an electrochemical method for the selective detection of Fe3+ ions. Therefore, the distinctive behavior of the heteroatom-doped GQDs provides a novel research platform for real-time applications in environmental safety and control.
Fig. 11 (a) Schematic diagram for charge transfer mechanism of CdS/Au/GQDs composite in (i) absence of dopamine (DA) and (ii) presence of DA, (b) variation in photocurrent response with the addition of different concentration of DA, and (c) calibration plot for the detection of DA by using CdS/Au/GQDs photoelectrode.133 Part (a), (b), and (c) are reproduced from ref. 133 with permission from [Elsevier], copyright [2020]. |
Nowadays, heteroatom doping of GQDs has developed as an appropriate approach for improving the properties of GQDs. But heteroatom doped GQDs still have some limitations such as they are mostly blue or green emissive under UV light irradiation, decrease in the PL intensity when emission peak is shifted towards higher wavelength and purification of GQDs. Also, the synthesis of uniform-sized GQDs is still a challenge. Mostly the reported methods give short scale-production of heteroatom doped GQDs but there is a need to produce them on a large scale. Further, the synthesis of heteroatom doped GQDs by simple methods and efficient purification techniques with different sizes is in great demand at the current time. The PL mechanism of heteroatom doped GQDs is still in debate. So, the theoretical calculations can provide an approach to understand the exact PL mechanism. Heteroatom doped GQDs have been used as various types of sensors such as PL, ECL, and electrochemical sensors based on different mechanisms. These sensors showed many advantages over the traditional sensors. But some of the sensors based on heteroatom GQDs showed drawbacks, for example, long fabrication process, pH and temperature dependent detection, long incubation time, complex process, etc. The removal of these drawbacks has become a future challenge. By eliminating these obstacles, the heteroatom doped GQDs become more prominent in the various fields.
This journal is © The Royal Society of Chemistry 2021 |