Jielong Wu†
,
Liangcai Wang†*,
Huanhuan Ma* and
Jianbin Zhou*
College of Materials Science and Engineering, Nanjing Forestry University, Nanjing, 210037, China. E-mail: wangliangcai@njfu.edu.cn; mahuanhuan@njfu.edu.cn; zhoujianbin@njfu.edu.cn
First published on 27th October 2021
To further understand the element migration characteristics and product properties during biomass pyrolysis, herein, pine cone (PC) cellulose and PC lignin were prepared, and their pyrolysis behavior was determined using thermogravimetric analysis (TGA). Subsequently, the PC was pyrolyzed in a vertical fixed bed reactor system at 400–700 °C for 60 min. The characteristics of element migration and the physicochemical properties of the pyrolysis products were analyzed and discussed. In the pyrolysis temperature range from 200 °C to 500 °C, there were two distinct weight loss peaks for PC. During the pyrolysis process, the C element was primarily retained in the biochar, while the O element mainly migrated into liquid and gaseous products in the form of compounds such as CO2, CO, and H2O. Besides, 28.42–76.01% of the N element in PC migrated into biochar. Of the three-phase products, the gases endow the lowest energy yield, while the energy of the biochar dominates the pyrolysis of the PC. Additionally, the N content and specific surface area for the PC-derived biochar obtained at 400 °C in a N2 atmosphere were higher than those of the biochar derived from fiberboard.
Previous works have indicated that the release of CO2 and CO during low-temperature (200–350 °C) pyrolysis (viz. torrefaction) of biomass allows for the elimination of oxygen faster than that caused by pure dehydration.8–15 Recently, numerous studies have shown that torrefaction can increase the carbon content and calorific value of biomasses, and reduce their oxygen content.16–19 According to these, we can conclude that torrefaction leads to changes in the content of O and C elements, especially the O element. In other words, torrefaction causes the migration of O and C elements from biomass. Notably, most of the biomass torrefaction research has focused on the solid products of biomass, and the physiochemical changes, fuel properties, and further uses of torrefied biomass have been extensively reported.20,21 In fact, in addition to the solid products, there are small amounts of gaseous and liquid products.22,23 However, relatively few systematic studies have been performed on the migration laws of carbon and oxygen elements as the collection of small amounts of gaseous and liquid products is difficult. Biomass pyrolysis (400–800 °C) can significantly increase the yield of gaseous and liquid products.
On the other hand, previous studies have indicated that the doping of carbon-based materials with other heteroatoms (e.g., N, P, and S) can further improve their properties.24–26 Schnucklake et al.27 synthesized nitrogen-doped porous carbon using phenolic resin as the carbon source and pyrrole-2-carboxaldehyde as the nitrogen source. It was presented that the nitrogen-doped porous carbon shows promising activity for the positive side reaction. Laheäär et al.28 used ammonia gas as the nitrogen source to modify activated carbon and indicated that the nitrogen-doped activated carbon with a nitrogen content of 4.50 wt% and a specific capacitance of 152 Fg−1. Xu et al.29 obtained biochar with 3.16 wt% N content by pyrolyzed the fiberboard containing phenolic resin. It was found that the biochar derived from fiberboard had a better adsorption effect on tetracycline. These previous studies have made significant progress in understanding that doped with N can enhance the active site of carbon. However, exogenous nitrogen (e.g., pyrrole-2-carboxaldehyde, ammonia gas, and phenolic resin) doping is not conducive to the uniform distribution of nitrogen in carbon materials, accompanied by the high cost. Therefore, biomass feedstocks with high nitrogen possess the potential to address the problem of uneven nitrogen doping and improve the active site of biomass-derived carbon. It follows that the nitrogen migration laws during pyrolysis of biomass feedstocks with high nitrogen are worthy of prior investigation.
Interestingly, pine cone (PC) is rich in nitrogen as an agroforestry waste, which is higher than that of other biomass like rice straw and grape stem, as well as is abundant in China.7,13 However, until now, most of the research on PC has focused on the development and investigation of natural medicinal extracts.30 Consequently, the pyrolysis behavior of PC and the migration law of C, O, and N elements in the pyrolysis process have not been reported yet. In the present work, the physicochemical properties for biochar, liquid, and gaseous products generated at different temperatures were determined via proximate analysis, ultimate analysis, Karl–Fischer titration, and so on. Overall, this work has made further understand of the deoxygenation, decarbonization, and denitrogenation from PC during pyrolysis at different temperatures.
Approximately 30 g of PC was placed into the reactor, and before the experiment, the reactor was purged with nitrogen to remove air from the reactor, and then the nitrogen was turned off after 10 min. Subsequently, the operating parameters (temperatures) of the vertical fixed-bed reactor system were varied to examine the properties of biochar, liquid, and gaseous products at a residence time of 60 min. During the pyrolysis process, the biochar remained in the reactor. Meanwhile, the liquid and gaseous products were collected in a liquid collecting device and a gas collecting bag, respectively. The pyrolysis experiment was repeated 3 times under the same experimental conditions to obtain enough products for subsequent testing. Besides, the volume concentration of each gas in the gaseous product was determined by a gas analyzer (Gasboard, Ruiyi Automatic Control Co., Ltd, Hubei, China).
The water content, pH, ultimate analysis, and composition of liquid were determined via Karl Fischer titration (KF-200, Mitsubishi Corporation, Japan), pH tester (E-201-C, Precision Scientific Instruments Co., Ltd, Shanghai, China), an element analyzer, and gas chromatography-mass spectrometry (Trace DSQ II, Thermo Scientific, USA), respectively.
(1) |
(2) |
A notable difference was found in the pyrolysis behaviors of PC, PC cellulose, and PC lignin. The weight loss of PC happens early in the temperature ranging from 110 °C to 200 °C. Moreover, the DTG curve of PC endows two distinct weight loss peaks in the pyrolysis temperature ranging from 200 °C to 500 °C, at around 330 °C and 450 °C, respectively. Of these, the weight loss peak at about 330 °C was caused by the pyrolysis of lignin or hemicellulose, while the weight loss peak at about 450 °C was primarily ascribed to the existence of non-structural substances (e.g., wax, fat, resin, tannin, sugars, and pigments). This is significantly different from other biomass shown only one peak such as bamboo,31 pinewood,32 and wheat straw,33 while similar to palm kernel had two weight loss peaks.8 The weight percentage for the pyrolysis residue of PC being ∼26%, which was consistent with the proximate analysis of PC (Table 1). Compared with the PC, PC cellulose was pyrolyzed in the lower temperature ranging from 200 °C to 380 °C and endows a narrow range of maximum weight loss upon 220–370 °C. Meanwhile, the weight percentage for pyrolysis residue was ∼23%. Unlike the sharper DTG peaks of PC and PC cellulose, PC lignin was slowly pyrolyzed in the wider temperature ranging from 160 °C to 700 °C and generated the highest weight percentage for residue (∼40%), this result was similar to the previous publication.8 Thence, the thermal stability of samples was determined: PC lignin > PC > PC cellulose.34
Samples | Proximate analysis (wt%, db) | Ultimate analysis (wt%, db) | HHV (MJ kg−1) | Energy yield (%) | ||||||
---|---|---|---|---|---|---|---|---|---|---|
Volatile | Fixed carbon | Ash | C | H | N | S | O | |||
PC | 73.98 ± 0.95 | 23.41 ± 0.44 | 2.61 ± 0.26 | 43.99 ± 0.49 | 3.65 ± 0.05 | 1.67 ± 0.07 | 0.51 ± 0.02 | 47.57 ± 0.89 | 17.86 ± 0.52 | 100 |
PPC-400 | 20.46 ± 0.77 | 71.69 ± 0.46 | 5.70 ± 0.32 | 66.11 ± 0.52 | 2.21 ± 0.04 | 2.79 ± 0.06 | 0.79 ± 0.03 | 22.40 ± 0.97 | 28.92 ± 0.59 | 73.68 |
PPC-500 | 16.57 ± 0.81 | 75.30 ± 0.49 | 7.99 ± 0.29 | 70.63 ± 0.48 | 1.09 ± 0.06 | 1.72 ± 0.05 | 0.53 ± 0.01 | 18.04 ± 0.89 | 29.68 ± 0.45 | 54.39 |
PPC-600 | 11.99 ± 0.87 | 79.47 ± 0.51 | 8.61 ± 0.34 | 74.07 ± 0.55 | 0.63 ± 0.03 | 1.65 ± 0.07 | 0.20 ± 0.02 | 14.84 ± 1.01 | 30.08 ± 0.65 | 51.01 |
PPC-700 | 9.48 ± 0.79 | 81.15 ± 0.45 | 8.96 ± 0.27 | 74.63 ± 0.51 | 0.53 ± 0.04 | 1.63 ± 0.06 | 0.15 ± 0.01 | 14.10 ± 0.88 | 30.31 ± 0.63 | 49.42 |
It is well known that the weight loss of PC during pyrolysis primarily resulted from the evaporation of volatiles. Fig. 4 shows the product distribution of the PC pyrolysis at different temperatures.
From Fig. 4, it can seem that an increase in pyrolysis temperature, resulting in an outstanding reduction in the yield of biochar, but the yield of liquid presented a gradual increase. Meanwhile, the yield of gas has no significant difference.
The weight loss gradually increased with the pyrolysis temperature from 400 °C to 700 °C, and had a relatively considerable weight loss (70.88%) at 700 °C, since the hemicellulose, cellulose, lignin, and non-structural substances of PC strongly decomposed.36 However, the increase in weight loss gradually slows down as the pyrolysis temperature increases. The sum of the yield of liquid and gas increased as the pyrolysis temperature increases, which was mainly attributed to the thermal cracking and lead to the formation of more volatiles.37 The effect of pyrolysis temperature on PC mass yield was similar to the effect on other biomass (e.g., cotton stalk, eucalyptus, and rice husk).38–40
The pyrolysis temperature has a notable effect on the physicochemical properties of biochar. The content of volatile gradually decreased as the pyrolysis temperature increases, such as 20.46% for PPC-400 and only 9.48% for PPC-700. Conversely, as the pyrolysis temperature increases, the ash content increased as a result of the ash remaining in the PC. Meanwhile, the content of fixed carbon equally increased significantly. Similar results were obtained for coffee chaff41 and Japanese cedar.42 This suggests that the pyrolysis temperature resulted in lower volatile content, while the higher ash content was due to enhanced thermal decomposition for the PC. In addition, the nitrogen content of PPC-400 was higher, which was 2.79%, and the nitrogen content was over those of other biochar such as coffee chaff biochar,41 rick husk biochar,43 and date seeds biochar.44 However, the nitrogen content of PPC-400 was similar to that of fiberboard biochar.29 In reviewing the literature, Li et al.45 indicated the nitrogen content of bamboo biochar detected by element analyzer and XPS being 0.6% and 0.4%, respectively. Wang et al.46 demonstrated the nitrogen content for lignin-derived porous carbon determined by element analyzer and XPS is 0.24% and 0%, respectively. Similarly, Xu et al.29 illuminated the nitrogen content for fiberboard biochar detected by element analyzer and XPS being 3.42% and 2%, respectively. Notably, the nitrogen element content detected by an element analyzer is higher than the nitrogen element content detected by XPS. A plausible explanation for this result can be given as follows: element analyzer and XPS work on different principles. For the elemental analyzer, the element content of samples is determined by the detector after combustion, secondary combustion, reduction, and interference gas removal, while XPS according to Einstein's photoelectron effect to determines the elemental content on the surface of samples. In other words, ultimate analysis demonstrates the elemental composition of samples, while XPS determines elemental content on the surface of samples. As such, when discussing the migration law of the N element, the N element determined by XPS will not be discussed if not mentioned otherwise.
Fig. 5 shows variation in H/C, O/C, and N/C element rations for the PC and biochar along with pyrolysis temperature.
With an increase in pyrolysis temperature, the element ratios of N/C increased at first, and then they slowly decreased and tended to be stable. However, the element ratios of H/C and O/C for the biochar gradually decreased as the pyrolysis temperature increases. This indicates that large amounts of H and O elements were removed from the PC, while the C element was enriched during the pyrolysis process. Compared to the ranges of the H/C and O/C element ratios found in the previous publication for lignite, peat, bitumen, and anthracite, the PC contains more O and H elements than all coals.47
Samples | Ultimate analysis (wt%) | Water content of liquid (wt%) | pH | HHV (MJ kg−1) | Energy yield (%) | |||
---|---|---|---|---|---|---|---|---|
C | H | N | O | |||||
a L-XXX stands for liquid obtained from pyrolysis of PC at XXX temperature. | ||||||||
L-400 | 8.21 ± 0.32 | 4.76 ± 0.03 | 0.62 ± 0.03 | 86.41 ± 0.62 | 73.03 ± 1.32 | 3.25 ± 0.27 | 10.40 | 16.80 |
L-500 | 7.99 ± 0.41 | 6.13 ± 0.04 | 0.64 ± 0.02 | 85.24 ± 0.53 | 74.56 ± 1.27 | 3.71 ± 0.32 | 7.89 | 17.60 |
L-600 | 7.76 ± 0.35 | 5.41 ± 0.05 | 0.81 ± 0.03 | 86.02 ± 0.57 | 76.45 ± 1.36 | 4.08 ± 0.38 | 8.74 | 20.60 |
L-700 | 7.82 ± 0.31 | 4.92 ± 0.03 | 0.92 ± 0.04 | 86.34 ± 0.62 | 77.89 ± 1.32 | 4.42 ± 0.29 | 10.12 | 24.54 |
Liquid had a C content of 7.76–8.21% and an O content of 85.24–86.41%. Meanwhile, with an increase in pyrolysis temperature, the water content of liquid gradually increased from 73.03% to 77.89%. This result suggests that increased temperature promotes the dehydration reaction. Besides, with an increase in pyrolysis temperature, the pH also increased from 3.25 to 4.42. This was mainly due to the water content of liquid gradually increased.
To compare the composition of the liquids obtained at different temperatures, L-400 and L-700 were subjected to GC/MS tests. As is known, the chromatographic peak area of a compound is considered to be linearly related to its content. Several representative compounds were selected as their comparatively higher peak area%. Table 3 lists the 30 components of L-400 with a relative content above 0.15%. Similarly, Table 4 exhibits the 34 components of L-700 with a relative content above 0.15%.
Time (min) | Relative content (%) | Compound name | Molecular formula |
---|---|---|---|
5.774 | 17.12 | Acetic acid | C2H4O2 |
11.961 | 9.08 | Furfuryl alcohol | C5H6O2 |
18.256 | 5.21 | Guaiacol | C7H8O2 |
17.945 | 4.23 | Phenol | C6H6O |
12.130 | 2.78 | 2-Methyl-2-cyclopenten-1-one | C6H8O |
10.411 | 2.13 | 2-Cyclopentenone | C5H6O |
20.411 | 1.95 | p-Cresol | C7H8O |
15.185 | 1.92 | 3-Methyl-2-cyclopenten-1-one | C6H8O |
8.704 | 1.89 | Pyrrole | C4H5N |
8.415 | 1.86 | Cyclopentanone | C5H8O |
12.632 | 1.81 | 3-tert-Butylcyclobutene | C8H14 |
8.049 | 1.65 | Propionic acid | C3H6O2 |
16.734 | 1.62 | 2,3-Dimethyl-2-cyclopenten-1-one | C7H10O |
19.309 | 1.59 | o-Cresol | C7H8O |
21.169 | 1.57 | 2-Methoxy-4-methylphenol | C8H10O2 |
15.338 | 1.53 | 2,3-Dimethyl-butane | C6H14 |
6.522 | 1.21 | Hydroxyacetone | C3H6O2 |
23.433 | 1.12 | 4-Ethyl-2-methoxyphenol | C9H12O2 |
9.484 | 1.09 | Dimethylmalonic acid | C5H8O4 |
6.615 | 1.03 | 2,4-Pentadienenitrile | C5H5N |
21.633 | 1.01 | 2,4-Dimethylphenol | C8H10O |
15.561 | 0.89 | 3,4-Dimethyl-2-cyclopenten-1-one | C7H10O |
7.378 | 0.85 | 2-Methyl-2-pentanol | C6H14O |
14.918 | 0.80 | 2,3-Dimethyl-2-cyclopenten-1-one | C7H10O |
9.670 | 0.72 | 2-Methylcyclopentanone | C6H10O |
17.007 | 0.58 | 2,3,4-Trimethyl-2-cyclopenten-1-one | C8H12O |
22.332 | 0.41 | Maltose | C6H6O3 |
8.234 | 0.34 | 4-Methylphenol | C7H8O |
13.758 | 0.22 | Phenol | C6H6O |
22.243 | 0.16 | Hydroxycarbamide | CH4O2N2 |
Time (min) | Relative content (%) | Compound name | Molecular formula |
---|---|---|---|
1.769 | 11.88 | Acetic acid | C2H4O2 |
12.893 | 8.92 | 1-2-Benzenediol | C6H6O2 |
10.492 | 4.36 | Valeraldehyde | C5H10O |
13.604 | 3.38 | 4-Methylcatechol | C7H8O2 |
5.150 | 2.46 | 2-Furan methanol | C5H6O2 |
11.248 | 1.96 | 3-Hydroxypyridine | C5H5ON |
1.589 | 1.94 | 2-Thiourea | CH4N2S |
2.229 | 1.89 | 3-Hydroxypropionic acid | C3H6O3 |
2.149 | 1.68 | Acetoxyacetic acid | C4H6O4 |
8.977 | 1.38 | 2-Hydroxy-3-methylcyclopent-2-enone | C6H8O2 |
6.406 | 1.34 | 2-Methyl-2-imidazoline | C4H8N2 |
10.282 | 1.20 | Guaiacol | C7H8O |
8.497 | 1.14 | N-Methylpiperidine | C6H13N |
8.056 | 0.63 | Phenol | C6H6O |
10.903 | 0.45 | 3-Ethyl-2-hydroxy-2-cyclopenten-1-one | C7H10O2 |
18.486 | 0.43 | Lauric acid | C12H24O2 |
10.808 | 0.40 | Maltose | C6H6O3 |
15.750 | 0.37 | 4-Ethylresorcinol | C8H10O2 |
6.516 | 0.36 | 4-Hydroxybutyric acid | C4H8O3 |
7.656 | 0.36 | 2,4-Dimethylfuran | C6H8O |
1.534 | 0.35 | Hydroxycarbamide | CH4O2N2 |
12.458 | 0.35 | 2-Methoxy-4-(methoxymethyl)phenol | C9H12O3 |
5.450 | 0.32 | Acetonyl acetate | C5H8O3 |
9.572 | 0.31 | Gamma-valerolactone | C5H8O2 |
10.082 | 0.31 | 4-Methylphenol | C7H8O |
17.980 | 0.31 | 4-Hydroxy-3-methoxyphenylacetone | C10H12O3 |
13.879 | 0.27 | 4-Hydroxy-3-methoxystyrene | C9H10O2 |
13.984 | 0.27 | m-Dihydroxybenzene | C6H6O2 |
7.846 | 0.25 | Dibuthylamine | C8H19N |
19.751 | 0.24 | Homovanillic acid | C9H10O4 |
1.564 | 0.18 | Isopropylamine | C3H9N |
7.001 | 0.17 | 3,5-Lutidine | C7H9N |
8.822 | 0.17 | 1,2,5-Trimethylpyrrole | C7H11N |
6.606 | 0.16 | 2,6-Dimethylpyrazine | C6H8N2 |
Table 3 indicates the top 5 products were acetic acid (17.12%), furfuryl alcohol (9.08%), guaiacol (5.21%), phenol (4.23%), and 2-methyl-2-cyclopenten-1-one (2.78%). Table 4 lists the top 5 products were acetic acid (11.88%), 1-2-benzenediol (8.92%), valeraldehyde (4.36%), 4-methylcatechol (3.38%), and 2-furan methanol (2.46%).
The liquids (i.e., bio-oils) are intensely complex in composition and contains an army of compounds. Although they were not likely to identify each ingredient, the liquids can be divided into several main categories according to the functional groups determined by GC/MS: acids, phenols, ketones, esters, alcohol, N-containing compounds, aldehydes, sugar, and furans. Total content for liquids ranged from 68.37% for L-400 to 50.19% for L-700, resulting from some components present in liquids were not calculated. The main components of L-400 and L-700 are shown in Fig. 6(a) and (b), respectively.
As seen in Fig. 6(a), the relative contents of acids, phenols, ketones, alcohols, N-containing compounds, and sugar were 19.86%, 17.27%, 13.30%, 11.14%, 3.08%, and 0.41%, respectively. However, the relative content of sugar was below 1.00%. Compared with L-400, L-700 (as indicated in Fig. 6(b)) had fewer acids and more N-containing compounds, which is consistent with the results of the PH as well as the ultimate analysis. Notably, the composition of L-700 is more complex than that of L-400, which suggests the high temperature leads to the secondary decomposition of many substances.
The gaseous products were primarily CO2, CO, CH4, and H2, which are derived from the decomposition of cellulose, hemicellulose, and lignin, and the mechanisms of their formation have been reported in the previous work.48 Of these, CO2 endows the highest volume concentration, followed by CO and CH4, but pyrolysis temperature was 700 °C, the CH4 volume concentration slightly more than the volume concentration of CO. With an increase in pyrolysis temperature, the CO volume concentration and the CmHn volume concentration have no significant difference, while the CH4 volume concentration and H2 volume concentration gradually increased. In reviewing the literature, CH4 is mainly derived from the pyrolysis of methoxy, methyl, and methylene in lignin.49 This suggests an increase in pyrolysis temperature, resulting in the lignin intensely decomposition, and produce more CH4, which coincides with the change of CH4 volume concentration in this study. HHV for the gases of 400 °C, 500 °C, 600 °C, and 700 °C was 4.93 MJ kg−1, 7.81 MJ kg−1, 11.19 MJ kg−1, and 13.68 MJ kg−1, respectively. These results manifested that with an increase in pyrolysis temperature, the heating values of gaseous products gradually increased.
When the pyrolysis temperature increased from 400 °C to 700 °C, the proportion of O in biochar decreased from 24.42% to 8.63%. Similarly, the proportion of O in gaseous products decreased from 26.30% to 12.76%. In contrast, the proportion of O in liquid products increased from 52.28% to 78.13%. This means that higher temperatures intensified the deoxygenation reaction. Element O was removed from the PC and migrated into the liquid and gaseous products in the form of CO, H2O, CO2, and oxygen-containing organic compounds. Notably, element O in PC was primarily transferred into H2O, followed by CO2 and CO. These results suggest that water and gaseous products play a vital role in deoxygenation.
When the pyrolysis temperature increased from 400 °C to 700 °C, the proportion of C in liquid products increased from 5.37% to 7.70%. Similarly, the proportion of C in gaseous products increased from 25.89% to 42.90%. In contrast, the proportion of O in biochar decreased from 68.38% to 49.40%. These results show that the C loss in PC was less than 50.60% over the pyrolysis temperature range. Meanwhile, with an increase in pyrolysis temperature, the proportion of N decreased from 76.01% for PPC-400 to 28.42% for PPC-700. As a result, the pyrolysis process of PC being a deoxygenation process along with C and N elements migration.
With an increase in pyrolysis temperature, the energy yield of biochar gradually decreased from 73.86% for PPC-400 to 49.42% for PPC-700, but the energy yield of liquid increased from 18.60% (400 °C) to 24.54% (700 °C). Among the three-phase products, the gases endow the lowest energy yield because it has the lowest mass yield. Notably, the energy of the biochar dominates the pyrolysis of the PC, which was consistent with the previous study.50
Samples | Surface area (m2 g−1) | Pore volume (cm3 g−1) | Average pore size (nm) | Nitrogen content (%) | Tetracycline removal efficiency (%) | Reference |
---|---|---|---|---|---|---|
a BCXXX stands for biochar derived from pyrolysis of fiberboard prepared at XXX °C, XXX can be 300, 500, and 800. | ||||||
BC300a | 32.2 | 0.022 | 2.5 | 3.54 | 55.45% | 29 |
BC500a | 34.9 | 0.033 | 4.3 | 3.16 | 63.29% | |
BC800a | 135.1 | 0.108 | 3.3 | 3.42 | 68.60% | |
PPC-400 | 65.3 | 0.066 | 2.0 | 2.79 | Further investigation | This study |
PPC-N-400 | 246.4 | 0.230 | 1.9 | 3.98 |
Consequently, we can infer that the PPC-400 and PPC-N-400 have potential in the field for removing tetracycline. Particularly, PPC-N-400 had a significant removal effect, and its removal efficiency may be over 68.60%.29
Footnote |
† These authors contribute equally to this work. |