Fyodor Malchik*a,
Kaiyrgali Maldybayeva,
Tatyana Kana,
Saule Kokhmetovaa,
Andrey Kurbatova,
Alina Galeyevaa,
Nufar Tubulb,
Netanel Shpigel
c and
Thierry Djenizianad
aAl-Farabi Kazakh National University, Center of Physical–Chemical Methods of Research and Analysis, Almaty, 050012, Kazakhstan. E-mail: Frodo-007@mail.ru
bDepartment of Chemistry and BINA – BIU Center for Nanotechnology and Advanced Materials, Bar-Ilan University, Ramat-Gan 5290002, Israel
cInstitute of Chemistry, The Hebrew University of Jerusalem, Jerusalem 9190401, Israel
dMines Saint-Etienne, Center of Microelectronics in Provence, Flexible Electronics Department, 13541, Gardanne, France
First published on 29th March 2022
The lack of stable electrode materials for water-based electrolytes due to the intercalation and conversion reaction mechanisms encourage scientists to design new or renovate existing materials with better cyclability, capacity, and cost-effectiveness. Ag4[Fe(CN)6] is a material belonging to the Prussian blue family that can be used, as its other family members, as an electrode material with the intercalation/deintercalation reaction or conversion-type mechanism through Ag oxidation/reduction. However, due to the instability of this material in its dry state, it decomposes to AgCN and a Prussian blue residual complex. A possible reason for Ag4[Fe(CN)6] decomposition is discussed. Nevertheless, it is shown that the decomposition products of Ag4[Fe(CN)6] have electrochemical activity due to the reversible oxidation/reduction of Ag atoms in water-based electrolytes.
Previous works have mostly been devoted to the electrochemistry of hexacyanoferrates, where a C-coordinated Fe reversibly shows an oxidation state varying between III and II in the potential range of 0.2–1.2 V vs. SHE (3.25–4.25 V vs. Li/Li+). The exact value of the working potential depends on the inductive effect of the N-coordinated transition metal ion, which make Prussian blue analogues (PBAs) ideal positive electrode materials for organic and water-based electrolyte metal-ion batteries. To compensate for the charge changes that occur during iron oxidation/reduction, a simultaneous intercalation/deintercalation of positive ions (Li+, Na+, K+, Ca2+, Al3+, etc.) occurs in the crystal lattice.5 There is also a wide scope of other PBAs with different C-coordinated transition metals (not only Fe) with broader values of standard potentials, which can be used as anodes for organic and water-based electrolyte batteries that present inherent reversible intercalation/deintercalation reactions of certain positive ions.2
In addition to the intercalation/deintercalation charge storage mechanism, there is a conversion reaction type for certain representatives of PBAs that are only used as anode materials and solely in organic electrolytes.6 The reason for this is the need for the application of low potentials, i.e. −3.05 to −1.45 V vs. SHE (0 to 1.5 vs. Li/Li+), to reduce Men+ to Me0 in PBAs. For example, in the case of one of the common cathode materials K2FeII[FeII(CN)6] during positive polarization (regarding OCV), there is a reversible potassium intercalation reaction (eqn (1)) with a practical capacity of 90 mA h g−1 at 0.1 A g−1 (∼1C) and good cyclability up to 1000 cycles (voltage window: 2.4–4.4 V vs. Li/Li+).7
K2FeII[FeII(CN)6] − K+ − e− ⇌ KFeIII[FeII(CN)6] − K+ − e− ⇌ FeIII[FeIII(CN)6] | (1) |
However, during negative polarization (versus OCV), there is a reversible conversion reaction forming metallic Fe (eqn (2)) that provides almost 400 mA h g−1 of initial capacity at 1C in a voltage range of 0 to 1.5 V (vs. Li/Li+) with the following slow degradation during 100 cycles (capacity retention: ∼50%).8
KFeIIFeIII(CN)6 + 5Li+ + 5e− ⇌ 2Fe0 + KCN + 5LiCN | (2) |
The demonstrated eqn (2) (ref. 8) is very simplified and in fact consists of several consecutive steps that should be investigated for a better understanding of the reaction mechanism.
One of the disadvantages of conversion reactions is the low reversibility of the 1st reduction process due to the full structure and morphology changes, and the formation of a surface electrolyte interface (SEI) leads to poor coulombic efficiency of around 50%.6,8,9 Another drawback is the low cycling life that is usually limited to 100–200 cycles with the capacity fading down to 50–70% compared to the 2nd cycle, which can be explained by the constant morphology changes followed by the loss of contact between the electrode and the current collector. Nevertheless, by applying a rational PBA representative, it is possible to achieve long cyclability at a high current density. It has been shown that KxMn[Fe(CN)6] has a multistep mechanism of conversion involving the fracture and recombination of Mn (N-coordinated) bonds, while the stronger Fe (C-coordinated) bond is still preserved (eqn (3)–(7)).6
KxMnIII/II[FeIII(CN)6] + xLi+ + xe− ⇌ Mn + Li5FeI(CN)6 + KCN + LiCN | (3) |
Mn + Li5FeI(CN)6 − 2e− − 2Li+ ⇌ Li3MnI[FeII(CN)6] | (4) |
Li3MnI[FeII(CN)6] − e− − Li+ ⇌ Li2MnII[FeII(CN)6] | (5) |
Li2MnII[FeII(CN)6] − e− − Li+ ⇌ LiMnII[FeIII(CN)6] | (6) |
LiMnII[FeIII(CN)6] − e− − Li+ ⇌ MnIII[FeIII(CN)6] | (7) |
The KxMn[Fe(CN)6]-based anode exhibits a reversible capacity of 480 mA h g−1 at a high current density of 1 A g−1 (∼2C) with a considerable cycling stability exceeding 1000 cycles, demonstrating that the right choice of transition metals in PBAs can significantly affect the reaction mechanism and its reversibility.
There are many examples of using conversion reactions in batteries with water-based electrolytes. Among them, silver–zinc and lead–acid batteries are the most famous and commercialized.10–14 Still, there is no electrode with a conversion type reaction based on PBA in water-based electrolytes due to the abovementioned reason of using low potentials (thermodynamic water instability). In this work, we study the possible application of the derivatives of the Prussian blue representative Ag4[Fe(CN)6].15 Ag4[Fe(CN)6] could potentially be used as an electrode material with the following reversible reaction (eqn (8)) (E0 = 0.1478 V vs. SHE).
Ag4[Fe(CN)6](solid) + 4e− ⇌ 4 Ag(solid) + [Fe(CN)6](soluble)4− | (8) |
However, the structural instability of Ag4[Fe(CN)6] in the dry state determined in this paper prevents its possible application. Nevertheless, here we show that derivatives obtained after Ag4[Fe(CN)6] decomposition with the inherent silver reduction/oxidation reaction have good reversibility in water-based electrolytes. The effect of certain cations and anions on the reaction reversibility of the synthesized material is investigated in detail.
Morphological characterization was conducted using a Magellan XHR 400L field emission scanning electron microscope (FE-SEM) (FEI Company) equipped with an energy dispersive X-ray spectroscopy (EDS) detector (Oxford Instruments).
The fact that there is no structural information on Ag4[Fe(CN)6] in the literature (though the compound is mentioned15), neither in the crystallohydrate nor water-free form, supports the hypothesised very low stability of the target compound. Apparently, Ag4[Fe(CN)6] is unstable at elevated temperatures (70 °C) or in a semi-dry atmosphere and loses structural water very easily. Considering that in most cases, Me4[Fe(CN)6]-type structures simply do not have enough space to accommodate four cations per single hexacyanoferrate anion in the PBA framework, stabilization can be achieved only by the introduction of water as an additional structural element of the framework, resulting in the general formula M4[Fe(CN)6](H2O)x (examples: K4[Fe(CN)6]·3H2O,20 Na4[Fe(CN)6]·10H2O (ref. 21)). Obviously, Ag4[Fe(CN)6](H2O)x does not have enough stability to hold the structural water and simply decomposes into AgCN.
From a practical point of view, it is still interesting to investigate the electrochemical properties of the synthesized material, such as the reaction reversibility, practical capacity, and stability, due to the probable existence of two electroactive phases: the conversion-type reaction of silver reduction/oxidation from AgCN (E0 = −0.017 V vs. SHE) (eqn (9)) and the cation intercalation in the remaining PBA derivative.
AgCN + e− ⇌ Ag + CN− | (9) |
SEM images of the synthesized material show the presence of nano-sized (50–100 nm) particles agglomerated into micron-sized boulders (Fig. 1 and S1†). The observed morphology of the complex material is not uniform without separation into 2 phases. EDX mapping of the material also confirms the presence of Fe, C, N, and Ag without indication of K, indicating a good washing process and having a good agreement with the XRD-detected components (Fig. S1†).
Electrochemical testing of the synthesized material was performed in LiCl and NaClO4 1 M solutions to check the reversible activity of the material for possible application in Li and Na aqueous batteries with different anions. The potential window was set from −0.75 to +0.75 V (vs. Ag/AgCl) to investigate the expected electrochemical reactions.
The CV curves show that the reduction peaks occurring at the first negative polarization are almost at the same potential (−0.214 V) in both electrolytes, revealing the same nature of the first electrochemical reaction (Fig. 2a). The peaks of the reverse process (oxidation) are found at different potentials: 0.121 V in LiCl and 0.157 V in NaClO4, suggesting the changing of the route of electrochemical reaction. The potentials of the subsequent reduction cycles in both electrolytes are different for each of the electrolytes and are shifted to a more positive value compared to the initial point. This potential shift can signify the decreasing overpotential of the same reaction due to the change in material resistance and the changing of the reaction mechanism, which will be discussed later. Furthermore, there is almost no capacity degradation in the LiCl electrolyte during 5 cycles, while there is a fast capacity fading with low reversibility at the 1st cycle in NaClO4 (capacity retention of the 1st cycle: 99.8% in the LiCl electrolyte, 40.9% in the NaClO4 electrolyte, Fig. 2b).
![]() | ||
Fig. 2 (a) CV curves of the synthesized material in 1 M LiCl and 1 M NaClO4 electrolytes at 5 mV s−1; (b) time capacity dependence curves obtained by CV curve integration. |
To investigate the different behaviour of the same material in two different electrolytes and understand the effect of electrolyte components (cations and anions) on capacity fading, post-mortem analysis of the electrodes after the 1st reduction (half cycle, charged) and after the reduction and oxidation processes (full cycle, discharged) was conducted by CV at 5 mV s−1 (Fig. S2†), followed by XRD and SEM analysis. The XRD and SEM experiments of the cycled electrodes were performed in a standard ex situ mode with the current collectors that affected the collected XRD data (additional intensive peaks of graphite foil, Fig. 3e).
SEM images of the electrodes after the electrochemical experiments in both electrolytes show significant differences in morphology and composition (Fig. 3a–d and S3†). After the first negative polarization to −0.75 V, a similar silver plating is observed on the electrodes. Both electrolytes (Fig. 3a and c) exhibit bright particles compared to the as-synthesized material (Fig. 1b). The process of silver plating occurs according to eqn (9) and should not be affected significantly by electrolyte cations and anions. However, major differences are visible after the reverse (oxidation) process to +0.75 V, wherein metallic silver should dissolve. In the case of the LiCl electrolyte, the morphology of the material fully returns to its initial state (Fig. 3b), while in the case of the NaClO4 electrolyte, dendrite-like particles form on the locations where metallic silver was plated (Fig. 3d).
To study the stability of the structures of the compounds on the electrode surface after the 1st reduction cycle, XRD analysis of the electrodes was performed. It showed that the formation of metallic silver occurs in both electrolytes similarly after charging up to −0.75 V (Fig. 3e, green lines). When discharged up to 0.75 V, the electrode material in the 1 M NaClO4 electrolyte system demonstrates no significant difference in the diffraction patterns between the 0.75 V and −0.75 V states, suggesting very little structural changes happening over the charge/discharge process. However, a closer examination of the diffraction pattern hints at the relative increase of AgCN peaks, suggesting the formation of additional amounts of this phase (Fig. 3e, green and violet lines). Considering the formation of dendrite-like particles seen in the SEM images, we can surely say that this is AgCN. New electrochemically formed AgCN starts to grow from metallic silver particles, and due to lack of CN− anions, (only released from the 1st charge, eqn (9)), dendrite-like particles are formed. Since metallic Ag is still present in the material, we may conclude the incompleteness of the Ag oxidation process. In the case of the material treated in the 1 M LiCl electrolyte system in the same conditions (fully discharged), we observe the vanishing of the Ag phase and the presence of the AgCl phase (Fig. 3e, black circles). Since the CV curves for the 1 M LiCl cell have significant stability over multiple cycles, we may conclude that the process is highly reversible. Despite the fact that the solubility constant is higher for AgCl (Ksp = 1.8 × 10−10) than for AgCN (Ksp = 2.5 × 10−16), the high concentration of chloride ions apparently promotes the formation of AgCl, which can be further cycled reversibly according to the following equation:
AgCl + e− ⇌ Ag + Cl− | (10) |
It should be noted that Fe4[Fe(CN)6]3(H2O)x does not undergo noticeable changes in the samples during the electrochemical reaction and dissolution in the electrolytes (Fig. 3e, blue line, PBA).
These findings show that the capacity degradation of the AgCN material in perchlorate electrolyte is conditioned by the lack of CN− diffusing to the electrolyte bulk (eqn (9)). Less than 41 wt% of the material is able to transform into the initial form after the 1st cycle following fast degradation. Meanwhile, there is negligible capacity fading in the chloride electrolyte due to the formation of AgCl and its known reversible reaction (eqn (10)).22,23
In order to check the cycling life and rate capabilities, the synthesized material was further investigated in 1 M LiCl electrolyte. The CV curves obtained at various scan rates (Fig. S4a†) demonstrate the high-rate capability of the conversion reaction (eqn (10)). Even at 50 mV s−1, there is 70% remaining capacity compared with the 1 mV s−1 case (79.7 and 114 mA h g−1, respectively, Fig. S4b†). Cycling stability tests of the synthesized material have been done by CV measurement (Fig. 4a) at 5 mV s−1, which revealed a 50.1% capacity fading up to 1000 cycles, which is fully confirmed by prolonged galvanostatic cycling (GC) at 1 A g−1 (10C, positive and negative voltage cut offs are +0.75 and −0.4 V, respectively). This also demonstrates 50.5% capacity degradation up to 500 cycles (Fig. 4b). We believe that the stability of the prolonged cycling conditioned only by Cl− ions does not depend on the cation (eqn (10)). This suggests the use of different soluble chlorides (Li+, Na+, K+).
![]() | ||
Fig. 4 Cycling stability tests of the synthesized material performed by (a) CV mode at 5 mV s−1 and (b) GC mode at 1 A g−1. |
Footnote |
† Electronic supplementary information (ESI) available. See DOI: 10.1039/d2ra00617k |
This journal is © The Royal Society of Chemistry 2022 |