Ayman Hijazi
*,
Nidal Khalaf
,
Witold Kwapinski
and
J. J. Leahy
*
Chemical and Environmental Science Department, University of Limerick, Limerick, V94 T9PX, Ireland. E-mail: j.j.leahy@ul.ie; Ayman.Hijazi@ul.ie; Tel: +353-83-3783841
First published on 6th May 2022
This review sheds light on the catalytic valorisation of agroforestry biomass through levulinic acid and formic acid towards γ-valerolactone and other higher-value chemicals. γ-Valerolactone is produced by the hydrogenation of levulinic acid, which can be achieved through an internal hydrogen transfer reaction with formic acid in the presence of catalyst. By reviewing corresponding catalysts, the paper underlines the most efficient steps constituting an integrated sustainable process that eliminates the need for external H2 sources while producing biofuels as an alternative energy source. Furthermore, the review emphasizes the role of catalysts in the hydrogenation of levulinic acid, with special focus on heterogeneous catalysts. The authors highlighted the dual role of different catalysts by comparing their activity, morphology, electronic structure, synergetic relation between support and doped species, as well as their deactivation and recyclability. Acknowledging the need for green and sustainable H2 production, the review extends to cover the role of photo catalysis in dissociating H2-donor solvents for reducing levulinic acid into γ-valerolactone under mild temperatures. To wrap up, the critical discussion presented enables readers to hone their knowledge about different schools and emphasizes research gaps emerging from experimental work. The review concludes with a comprehensive table summarizing the recent catalysts reported between the years 2017–2021.
The derived biomass molecules are symbolized by their functional groups, which facilitate their use in producing chemicals compared to saturated alkanes.11 LA is known for facilitating the production of added-value molecules. This can be achieved through its catalytic hydrogenation using secondary alcohols or FA as a H2 donor.12,13 Therefore, FA is a promising biomass-derived compound that presents a potential pool of energy source of H2.
Here in this review, we mainly focus on the valorisation of cellulosic food waste into LA and FA, as part of establishing sustainable production of higher-value chemicals and liquid fuels. The valorisation routes starting from cellulose and hemicellulose are defined in Section 2. Our approach is economic-oriented, and we seek to shed light on one-pot processes as presented in Section 3.2.1, wherein the in situ produced H2 via FA decomposition provokes the hydrogenation of LA into further useful compounds, eliminating the need for an external source of H2. The decomposition of FA into H2 is highlighted in Section 3.1 (Table 1), while an overview of different H2 sources is presented in Section 4, with an insight into the photocatalytic hydrogenation of LA into GVL using alcohol solvents presented in Section 4.1. To add, using H2 for hydrogenation reactions remains a challenging step as it possesses low mass transfer in many organic solvents.14 Heterogeneous catalysts featuring a dual role of dehydrogenation/hydrogenation for driving the above process are also emphasized in Sections 3.1 and 3.2 Table 2. Moreover, insight into the nature of catalysts that have been used to date is gained by relating activity, deactivation, and recyclability to their morphological structure, as shown in Section 3.2.1.
Catalyst | TOF (H2) | Solvent | Temp. (°C) | Ref. |
---|---|---|---|---|
a TOF: Turn over frequency (s−1). | ||||
Pd–P–SiO2 | 719 h−1 | Formate salts HCOONa | 85 | 36 |
Pd–S–SiO2 | 959 h−1 | K2SO4 | 85 | 36 |
Pd shell@Ag core | 252 h−1 | H2O | 50 | 40 |
Pd–Au/C | 27 h−1 | Formate salts HCOONa | 90 | 45 |
Pd–Au/C–CeO | 832 h−1 | Formate salts HCOONa | 102 | 38 |
Pd/γ-Al2O3 | 600 h−1 | NaOH, 0.1 vol% O2 | 20 | 52 |
1 wt% Pd/C | 255 h−1 | Gaseous phase | 100 | 46 |
Au/TiO2 | 201 h−1 | Gaseous phase | 100 | 50 |
Au/SiO2 | 7023 h−1 | Gaseous phase | 100–300 | 51 |
Finally, in Section 5, we highlight recent studies that suggest promising catalysts, enabling simple down streaming and upgrading of GVL into significant compounds such as pentanoic acids (PA). Ultimately, bio-solvents are the candidate final product to which further analysis could be done to substitute petroleum-derived solvents involved in pharmaceutical industries. Nevertheless, this review provides attention on gaps and challenges to shift individual catalytic reaction steps into a process that extends from upstream treatment of lignocellulosic biomass to higher value end products.
HCOOH → CO2 + H2 | (1) |
HCOOH → CO + H2O | (2) |
It was reported that both pathways are thermodynamically favoured. Indeed, both reactions are easily shifted forward due to negative Gibbs free energy of −32.9 kJ mol−1 and −20.7 kJ mol−1, respectively.28 The slight difference in Gibbs free energy as well as enthalpy results in competitive production of CO as a by-product, when H2 is targeted.29 Selective production of CO-free H2 is the ultimate goal to obtain an enhanced overall catalytic performance of LA hydrogenation via internal H2 transfer using FA. Therefore, designing a heterogeneous catalyst that favours dehydrogenation of HCOOH (eqn (1)) on the expense of the dehydration step (eqn (2)) is a key approach for LA/FA system to avoid unfavourable CO by-product, which leads to the poisoning of heterogeneous catalyst.30,31
FA decomposition in the presence of metals, alloys, and oxides heterogeneous catalysis dates back as far as the 1950s and 1960s.32 Heterogeneous catalytic systems were developed to seek appreciable reaction kinetics of FA decomposition while saving energy demand for the reaction. Generally speaking, noble metal heterogeneous catalysts favour dehydrogenation decomposition of FA (eqn (1)), whilst oxides and base metals catalysts are engaged in the dehydration route (eqn (2)).33–35 Zhao Y. et al. synthesized a group of immobilized catalysts by anchoring Ru and Pd metals using functionalized groups onto silica supports. Amongst, Pd–P–SiO2 attained the highest activity of TOF of 719 h−1 at 85 °C followed by Ru–S–SiO2 with TOF of 344 h−1. Decreasing temperature resulted in lower activity, which reached TOF of 16 h−1 for Pd–S–SiO2 at 45 °C. It was found that the inclusion of sulfates by using Na2SO4, MgSO4, and K2SO4, boosted the catalytic activity to exceed 940 h−1 with sulphur functionalized catalysts.36 These results bear Pd(II) as an active species, which is stabilized by mercaptopropyl groups.36 Nevertheless, performing FA decomposition in the presence of heterogeneous catalysts suffers from drawbacks owing to the presence of CO contamination, water vapour formation, and therefore catalyst deactivation.37,38 To illustrate, elevated temperature favoured decarbonylation reaction, generating CO gas despite using active Pd–Au/C core–shell catalyst.38,39 For this reason, Tedsree K et al. optimized a core–shell catalyst by the inclusion of core metal Ag into Pd shell metal to be active for FA decomposition at low temperatures. The attractive activity of TOF = 252 h−1 at 50 °C was observed for Ag@Pd (1:1) core–shell catalyst. This trait is attributed to altering Pd active sites via direct charge transfer from Ag core metal, which thereby stimulates the bridging adsorption of FA to promote hydrogen production.40 Further on bimetallic catalysts, the morphology is influenced by the followed preparation method. Bimetallic Pd–Au can be constructed as a mixture, clusters to clusters, random alloy, and core–shell.41,42 These options can be achieved through calcination. For instance, Pd is detected in the outer framework of the particle surface, resulting in a rich Pd shell on top of an Au rich core. This structure could be flipped by further calcination that leads to Pd rich core and Au rich shell morphology.43 Additionally, the application of subsequent calcination processes yields further structural changes signified by three shell layers of core–shell catalyst: Pd–Au alloy as the inner core, Au as intermediate layer, and a rich Pd outer shell.44 Haung Y. et al. prepared a core–shell Pd/Au@Au/C catalyst, which showed a high anti-poisoning activity versus CO and an attractive activity represented by 90% conversion of FA and only 30 ppm CO after 6 h at a temperature of 92 °C.39 Moreover, they proposed the crystallization process for making Pd/Au@Au/C system (Fig. 1).
Fig. 1 Crystallization process of Pd/Au@Au/C system.39 |
Another bimetallic catalytic system was studied by Zhou X. et al. in which they discovered that the highest FA dehydrogenation was attributed to Pd–Au alloy system as well as Pd–Ag alloy on a carbon support. Considering the loading ratio, reaction temperature and HCOOH/HCOONa ratio, Pd–Au/C showed the highest TOF of 27 h−1 followed by Pd–Ag/C with a value of 17 h−1 at 365 K. An attractive catalyst stability for 240 h−1 with only 80 ppm of CO formation is attributed to the basicity of HCOONa solution. The resulting reforming gas qualifies for PEMFC standard as it doesn't exceed 100 ppm CO.45 The inclusion of CeO into both catalysts improved their activity further due to the formation of more oxidized Pd that can oxidize adsorbed CO. Indeed, the TON attained was 227 h−1 and 76 h−1 for Pd–Au/C–CeO and Pd–Ag/C–CeO, respectively.38 The improved catalytic activity of TON of 832 h−1 was observed at a higher temperature of 375 K using Pd–Au/C–CeO alloy catalyst.
Bulushev et al. compared the activity of Pd and Au active sites over carbon and TiO2 supports in gaseous phase FA decomposition at 373 K. The highest TOF of 255 h−1 was attributed to 1 wt% Pd/C followed by 10 wt% Pd/C with a TOF of 180 h−1. The higher decomposition rate of FA was due to the higher dispersion of Pd nanoparticles. On the other hand, lower activities were observed for 1 wt% Au/TiO2 and 0.8 wt% Au/C at TOFs of 57 h−1 and 21 h−1, respectively. Despite the higher activity of Au/TiO2 catalyst in decomposing FA, a lower selectivity of H2 was noticed,46 which comes in agreement with TiO2 support engaged in favouring FA decomposition through decarbonylation route (eqn (1)).47,48 It was reported elsewhere in literature that Au comprises low areal rates in comparison with other noble metals, which is represented by first-order kinetic of FA decomposition,49 whereas well-dispersed Au is capable of decomposing FA.50 It is worthy to note that Pd particles were inhibited by CO which exhibits strong adsorption. Whereas, Au showed weaker CO adsorption and improved WGS reaction, producing additional H2.46 Further interesting work was done on investigating the role of Au species in FA decomposition. The thermal treatment of Au/Al2O3 caused Au cluster size to increase (sintering effect) accompanied by a drastic decrease in HCOOH decomposition rate. Consequently, FA dissociation is favoured by well spread Au species only. Despite similar cluster size of Au/TiO2 and Au/Al2O3 of 3–4 nm, the TOF for HCOOH decomposition were 201 mol h−1 g−1 and 7 mol h−1 g−1, respectively. In this context, Au is less dispersive over TiO2 than on Al2O3 support. It is worth noting that none of the used catalysts; Au/TiO2, Au/Al2O3, and Pt/Al2O3 yielded CO and H2O, indicating the absence of dehydration of HCOOH and reverse WGS reaction.50 On another end, the authors proposed that the irreversible production of H2 is achieved by the adsorbed H produced by the preceding step as shown below.50
(3) |
(4) |
Eqn (3) and (4) further studies investigated the catalytic performance of Au species over different oxide supports. Gazsi A. et al. found that Au/SiO2, Au/CeO2, and Au/Norit favoured FA decomposition through dehydrogenation route (eqn (1)). Whilst dehydration of FA (eqn (2)) was dominated in the presence of Au/Al2O3, Au/ZSM-5, and Au/TiO2. The most active catalyst regarding FA conversion was Au/SiO2 with a TOF 7023 h−1 of 100% H2 selectivity between 373 K and 523 K. They also reported that the FA rate of decomposition is not dependent on Au particle size.51 However, their results came in contrary to conclusions about the Au cluster size effect investigated by Manuel Ojeda and Enrique Iglesia as mentioned previously.50
Regarding reaction kinetics, FA decomposition follows a zero-order pattern over Au/SiO2, which depends on formate intermediates instead of HCOOH substrate initial quantities.51 This comes in harmony with the suggested kinetics by Ojeda M. et al. who also recognized that changing HCOOH partial pressure did not affect FA decomposition.50 In both studies, the proposed mechanisms involve the cleavage of C–H bond of formate, which falls in the rate-determining step.50,51 Another contradiction arises regarding H2 selectivity. A very low yield of H2 (TOFH2 = 18 h−1) was observed for Au/Al2O3 at 473 K,51 whereas much higher H2 was produced with only 10 ppm of CO traces detected in the presence of Au/Al2O3 at ambient temperatures.50 In both cases, Au inhibited catalyst deactivation due to weak CO–Aux complex formation.
A very recent breakthrough was achieved by Xu P. et al. on removal of adsorbed CO over Pd/γ-Al2O3 by adding traces of oxygen. The effect of the concentration of O2 on the conversion and selectivity of the FA decomposition was also investigated. The optimal concentration of O2 of 0.1 vol% yielded an activity of TOFH2 = 600 h−1 beyond which the selectivity of H2 drops down, while conversion was preserved at 60%. The yield of H2 dropped to 500 h−1 at O2 concentration of 2 vol% due to the consequent oxidation of H2 into H2O on the expense of CO oxidation.52 Sneka-Płatek O. et al. used another approach to inhibit CO poisoning in which tuning the alloy ratio of Ag:Pd at 4% Ag–1% Pd resulted in isolated Pd atoms and thereby in the highest conversion of HCOOH at 34%.53
Owing to the difficulty of handling conventional storage systems as an external source of hydrogen, shifting towards the in situ production of hydrogen from FA for hydrogenating reactions has become crucial.59,60
Biomass compounds processing has been well discussed in literature from different perspectives. A good review was published elsewhere about upgrading biomass-derived compounds from different cellulosic biomass fractions, e.g. cellulose, hemicellulose, and lignin through C–C coupling reactions (Fig. 2).3
Fig. 2 Biomass platform molecules upgrade into valuable products and fuel additives.3 |
Another review focuses on the conversion of carbohydrates using heterogeneous catalysts. For instance, hexoses and pentoses, the building rocks of carbohydrates, undergo dehydrogenation and dehydration catalytic reactions to yield HMF and furfural (Fig. 3), respectively, which are subsequently upgraded into fine chemicals.61
Fig. 3 Possible routes for dehydration of carbohydrates into levulinic acid and furfural platform compounds.61 |
Huber W. G. et al. wrapped up all known routes to produce bio-oils from lignocellulosic biomass. They reported a wide range of liquid fuels and gasoline additives that are formed through molecular weight adjustments.62
Levulinic acid has been widely reported as an attractive platform chemical from which higher-value chemicals are produced, including levulinate esters, GVL, HMF, and MTHF. Noteworthy, designing a process with the least number of deoxygenating steps as one-pot transformation is shifting to a more economic route. As an added advantage for a cost-effective biomass process, replacing the external source of hydrogen by in situ molecular H2 produced from FA is applied in addition to designing a catalyst capable of performing dehydrogenation and hydrogenation.
LA platform chemical along with FA is produced commercially from sugars that are produced subsequently from cellulose (Fig. 4). The production cost is estimated to be 0.09–0.11 $ per kg for a throughput of 1000–2000 dry tons per day.63
Fig. 4 Two-stage production of levulinic acid and formic acid from cellulose.63 |
LA comprises distinctive properties due to the presence of carbonyl and ketone functional groups. Consequently, LA can undergo different reactions, mainly at its carbonyl group to yield cyclic compounds. Owing to its distinct products including but not limited to GVL, levulinate esters, 2-methyltetrahydrofuran, valeric biofuels, and pentanoic acid.64
Deng Li et al. developed a catalytic route that comprises the production of GVL from biomass carbohydrates with a yield of 93 mol% by using RuCl3.3H2O/PPh3 with pyridine base at 423 K. The novelty is pronounced by eliminating the need to separate levulinic acid from FA in the intermediate mixture. Noteworthy, it was found that introducing CO2 to the reaction medium boosted the catalytic activity of Ru catalyst to reach a yield of 100 mol% GVL, whilst H2O did not have any effect.65
Sequential production of deoxygenated compounds is achieved by Ru/C catalyst followed by a dual catalytic bed containing Pd/Nb2O5 & Ce–Zr. The former catalyst completely converted LA and FA into GVL at 423 K. In the second reaction stage, Pd/Nb2O5 catalyst resulted in 100% conversion of GVL with 78% selectivity of pentanoic acid. Further on, they observed that the addition of zirconia led to further improvements. Indeed, the dual catalyst system Pd/Nb2O5 & Ce–Zr produced 89% selectivity of nonanone (C9) from GVL.66 Even though sulphuric acid was reported as a major inhibitor for catalysts, Ru/C catalyst showed good activity in the presence of H2SO4 medium.67,68 The authors explained this by emphasizing the importance of using optimum H2SO4 proportions for cellulose pretreatment during the upstream process.66
In another study done by Deng Li et al., their previous work including one-step process using RuCl3/PPh3 catalyst is substituted by two-step processes using immobilized Ru–P/SiO2 catalyst for FA dehydrogenation and Ru/TiO2 for intramolecular hydrogenation of LA into GVL. The immobilized Ru–P/SiO2 catalyst showed highest TOF of LA of 447 h−1 at 423 K (GVL yield 96%).69 However, the team encountered contradictory results with Ruiz et al.66 regarding the activity of Ru/C catalyst. According to Deng Li et al.,69 the Ru/C catalyst did not show promising results in FA decomposition and in situ hydrogenation of LA into GVL (TOF 69 h−1, 7% GVL yield). Instead, Ru/TiO2 catalyst exhibited 63% GVL yield from LA at 4 MPa H2 at 423 K.69 An important aspect of the effect of CO2 on Ru-catalysed hydrogenation of LA arose from this research; reinjecting the CO2 produced from FA did not show any improvement of Ru/C in catalysing LA hydrogenation.69 Dongmei H et al. (2017) also evaluated the activity of immobilized Shvo's catalyst over SiO2 surface as well as covalently grafted catalyst in reducing LA into GVL using FA while avoiding the external use of H2. The highest activity of 504 TON, 21 TOF(h−1) and 88% GVL yield was attributed to immobilized Shvo's catalyst over SiO2 surface. The reaction was held in the presence of 1,4-dioxane solvent under nitrogen gas for 24 h at 90 °C.70
Feng J. et al.71 proposed a new reaction pathway for the production of GVL from LA using FA solely as H2 source. A blend of Ru/C catalyst and trimethylamine accelerated LA hydrogenation and resulted in considerable activity at 87.26% as LA conversion and 80.75% as GVL yield. The XRD pattern showed an overlap between the characteristic peaks of Ru and graphite at 2q = 44.6°, implying the high dispersion of Ru over carbon support. The proposed reaction route was exhibited using experiment probe of HPLC, 1H NMR & 13C NMR by which LA, triethylamine, GVL, ethanol, 4-hydroxyvaleric acid, and ethyl levulinate are the compounds present at the end of the reaction. This features two important observations, the first of which is that FA was completely consumed, and that the esterification reaction is possible due to some produced ethanol that reacts with LA. The postulated mechanism is a good tool that helps researchers in investigating for the possible production of CO on the expense of CO2 from FA decomposition (Fig. 5).
Fig. 5 Proposed reaction pathway of LA into GVL and ethyl levulinate using FA.71 |
Due to the continued concern over the inhibiting effect of H2SO4 on heterogeneous catalysts,68,72 Heeres H. et al.22 proposed the use of TFA instead. It was reported that TFA has a pKa value of 0.5.73 Indeed, TFA resulted by a yield of 57 mol% of GVL22 slightly higher than the yield of GVL of 55 mol% in the presence of H2SO4.20 The team studied extensively the conditions of conducting a one-pot process starting from C6-sugars to yield GVL. It was found that Ru/C catalyst resulted in 11 mol% LA yield and 52 mol% yield of GVL.22 On another note, the authors also shed light on further improvement of GVL yield% while minimizing hydrogenation side reactions, which can be achieved by tuning reactor parameters; temperature and mixing.22 An alternative strategy to avoid catalyst inhibition by the acidic medium is using reactive extraction in which butene is added to LA, FA, and H2SO4 aqueous solution to yield formate esters and levulinate esters. The aforesaid aqueous solution is separated easily into an organic phase (hydrophobic esters) and pure H2SO4 upon its contact with water. The group proposed a dual catalytic system containing Pd/C followed by Ru/C catalysts. H2 is generated in situ from FA and formate esters over Pd/C hydrogenate LA and its ester over Ru/C catalyst.74 This comes in harmony with sulphur tolerant Pd support material used for catalysts.75,76
Interestingly, SnCl4 catalyst was used as a substitute for H2SO4 in breaking down furfural biomass carbohydrates into LA and FA, which subsequently undergo catalytic transfer hydrogenation over Au–Ni/ZrO2.77
Kopetzki D et al. suggested the use of Na2SO4 salt in reducing LA into GVL using H2 produced from FA. The salt catalyst activity relies on its dissociation constant in which SO 2−4 ions switch into a weak base at elevated temperatures (548 K) and eventually deprotonate FA. Hence, the use of a conventional base was avoided.78 It was reported elsewhere that salt additives induce autocatalysis in aqueous solutions.79 Accordingly, this approach should be given more attention towards either improving its activity further or blending it with other heterogeneous catalysts to boost up the GVL yield.
The high sensitivity of Ru/C catalyst amid acidic conditions inspired Demesic et al. to synthesize 15 wt% RuRe (3:4)/C catalyst for the hydrogenation of LA by FA in the presence of H2SO4, with no observed deactivation. Indeed, the utilized catalyst resulted in a GVL yield of more than 95% at 423 K and higher stability, which is demonstrated by the increased TOF from 50 h−1 to 150 h−1 for Ru/C and RuRe/C catalysts, respectively.6 Likewise, the concept of Ru/C catalyst deactivation due to presence of acids drove Cao et al. to study the catalytic hydrogenation of LA by consuming FA as a reducing agent using Au nanoparticles on different catalyst supports. Their results presented ZrO2 doped with Au as an attractive catalyst in comparison with Pd, Pt, Ru, and Pd as well as Au/C, Au/SiO2, and immobilized Au/TiO2.80 The activity of Au nanoparticles was linked to its particle size (1.2–2.5 nm). Both studies come in agreement regarding the particle size effect of Au particles; larger particle size has limited the activity of Au catalyst.50,80 Therefore, the good catalytic activity of Au nanoparticles over ZrO2 could be attributed to its value-added activity in HCOOH decomposition step.81 The high dispersion of Au nanoparticles of size 2.4 nm in their metallic state (Au0) was found to be improved by the inclusion of Ce into Au doped ZrO2 catalyst. These improvements play a key role in enhancing the decomposition of FA and thereby the hydrogenation of LA. The addition of Ce facilitated the formation of tetragonal phase of Zr along with the increase of weak and medium acidic sites, thus the formation of GVL was considerable at yield 83.5% due to upgraded dehydration reaction of the intermediate derived from LA hydrogenation reaction at conversion 90.8%. Despite the use of a high reaction temperature of 240 °C, the catalyst showed robustness with a limited decrease in its activity after 5 consecutive runs.82 Another study performed by Zhou C. et al.77 confirmed the improvement of Au/ZrO2 activity in hydrogenating LA by means of FA in the presence of highly dispersed Au0 due to the incorporation of Ni metal. The role of Ni comes in agreement with the above-mentioned Ce106 in reducing Au particles to provide highly dispersed doped Au0 with less aggregation.
A strong relation between the method of preparation of nano-alloy Ni-based Au doped catalyst and its activity in hydrogenating LA into GVL in the presence of FA was demonstrated by M. Ruppert A. et al. It was found that highest LA conversion and highest GVL yield at 89% and 86%, respectively, were attributed to co-impregnation method of both metal precursors which are then thermally reduced under H2. The group utilized DFT calculations and thorough characterization for the nano-alloy surface and concluded that selective FA decomposition is due to high energetic span of FA adsorption was favoured by Ni atoms incorporated within Au nanoparticles.83
The effect of Au nanoparticles on different oxidic supports was studied thoroughly on LA decomposition into GVL using hydrogen transfer reaction in the presence of FA. Different Au@oxides catalysts were synthesized using co-precipitation and conventional impregnation techniques. Various oxide supports including ZrO2, Al2O3, SiO2, TiO2, MgO were used for fabricating Au doped catalysts by which Au/ZrO2 achieved highest GVL yield of 85% and LA conversion of 93% at 210 °C after 5 h.84 Unlike Au–Ce/ZrO2 catalyst reported above,82 the presence of Au3+ species improved the activity of the catalyst. XPS analysis elucidated the decrease in Au3+ species from 49.2% in fresh catalyst to 10% in spent one due to reducing agent FA. The Au/ZrO2 catalyst synthesized by co-precipitation experienced a slight drop in GVL yield to 69% after 3 reaction runs.84
The activity of Ru/C showed the highest conversion values of LA into GVL, and the highest selectivity compared with Pd/C, RANEY® Ni, and Urushibara Ni. Nevertheless, Ru/C exhibited low stability which necessitates adding a portion of fresh catalyst for further runs. LA conversion and GVL selectivity dropped from 92% and 99% on its first run to 61% and 70% after the second run, respectively. Above all, the authors emphasized the hydrogenation mechanisms over Ru/C catalyst (Fig. 6).
Fig. 6 Levulinic acid hydrogenation mechanism over Ru/C catalyst.11 |
Both LA and H2 are chemisorbed on Ru/C before H–H bond cleavage step takes place, where one H atom will be transferred onto the carboxyl oxygen in LA and consequently an intermediate is produced. Thereafter, a second H atom transfers to the carbonyl carbon produces γ-hydroxyvaleric acid which undergoes subsequent dehydration into γ-valerolactone.11
Recently, Al Naji M. et al. made a breakthrough in the field of LA hydrogenation in the presence of FA as a reducing agent in aqueous solution. The novelty of their work was pronounced by synthesizing a robust catalyst, comprising high thermal stability and can withstand low pH conditions (pH = 2). The most active catalyst, 1.6 wt% Pt/MP-ZrO2 achieved a LA conversion of 84% and a GVL yield of 82% at 493 K after 24 h reaction time. Noteworthy, pentanoic acid of 22% wt was discovered at a higher temperature (533 K).85 On a different note, the authors confirmed that FA acid decomposition into H2 and CO2 is a rate-limiting step which precedes LA hydrogenation over the same Pt active sites (Fig. 7).
Fig. 7 Competitive FA dehydrogenation and LA hydrogenation over Pt active sites to GVL and PA.85 |
Their findings come in line with Gazsi et al.51 and Ojeda et al.50 as it proved that C–H bond cleavage contained by formate intermediates controls the overall reaction. To add, the reaction follows zero-order kinetics, same as mentioned in the literature, which can be attributed to the desorption of CO2 & H2 to the liberation of Pt active sites for LA hydrogenation (Fig. 7). This suggests a competitive adsorption between LA and FA on the active sites that provoke hydrogenation,31 featuring FA decomposition the rate limiting step of the overall reaction.
It was previously emphasized that TiO2 and ZrO2 supports resulted in good activity regarding LA conversion to GVL using external molecular H2 at 473 K.86 Whereas, ZrO2 exhibited higher activity and stability in comparison with TiO2 support when doped with Ru active sites.11,87 In this context, Al Naji et al. also synthesized a bifunctional catalyst by way of doping noble metal Pt on zeolite support. The discovered catalyst was characterized by its acidic property, which thereupon permitted its ability to convert GVL into pentanoic acid. Briefly, this conversion was accomplished via a moderate number of acidic sites of zeolite, on which GVL ring-opening into pentanoic esters is favoured. At the same time, PEAs are hydrogenated using H2 produced from FA decomposition, where both reactions (PEAs hydrogenation and FA decomposition) occurred over dual Pt active sites. The enhanced activity of hydrogenation/dehydrogenation reactions using dual active noble Pd metal supported on acidic zeolite catalyst were also demonstrated in pyrolysis of waste rubber, cracking down complex hydrocarbons into simpler compounds.88 The conversion of LA achieved via the dehydration of 4-hydroxypentanoic acid intermediate, which is considered as a rate determining step, was reportedly enhanced by tuning Zr/Al ratio of Ru/(AlO)(ZrO)n catalyst. The improved activity was characterized by enhanced strength and distribution of Lewis acidic sites of (AlO)(ZrO)0.1 and calcination temperature of 400 °C.89
Designing an economic LA hydrogenation system is shifting from using sustainable FA as a hydrogen donor alone to the use of inexpensive metal catalysts. For instance, non-noble metals were tested in LA hydrogenation in the presence of catalytic transfer hydrogenation using nickel, zirconium, and iron.90–93 Amongst, Zr comprises the required acidity that stimulates LA hydrogenation into GVL.94,95 This was characterized by the high LA conversion due to high acidic density sites (136 μmol g−1) when Zr was used as a support in 1.6 Pt/MP-ZrO2.85
Non-noble metals heterogeneous catalysts have always been an attractive topic for researchers as they seek cost-effective biomass hydrogenation processes. A recent study investigated the relation between the catalyst performance of MnCo oxide catalyst and its crystal structure. Series experiments were made using several MnCo oxide catalysts using different Mn:Co ratios. The highest activity corresponded to Mn2Co0.1Ox of 83.4% LA conversion and 70% GVL selectivity achieved at 230 °C. The improved activity was attributed to the structural distortion induced at MnCoO3 and MnOx interface, which facilitated the adsorption of FA by H–H formation and π–π interaction with ketone group of LA simultaneously. Previous attempts for applying non-noble metals in hydrogenating LA into GVL using FA in vapour phase96–101 and in aqueous phase102–108 are published elsewhere. Amongst, deactivation was studied by Hussain Sk et al.101 who found that using pure MgO catalyst exhibited good activity at the start-up before it declines due to deactivation. However, using calcined Mg–Al hydrotalcite catalysts yielded complete conversion of LA for 10 h and appreciable selectivity of GVL of 98%. The catalyst showed a good extent of stability conveyed by the reusability under same reaction conditions. The conversion of LA dropped to 86% while GVL selectivity was preserved near 98% after 4th cycle of the reaction.109
A recent study also aimed at designing cost-efficient catalyst that is effective in hydrogenating LA into GVL at mild reaction conditions. The group used hard-soft template-assisted electro-deposition method to engineer Ni78Pt22 nanowires based on polycarbonate membranes that accommodate Ni–Pt mesoporous wires. Experiments showed that a TOF of 74 h−1 (100% conversion) and GVL selectivity near 99% were achieved at 140 °C during 120 min110. Ni and Cu cheap metals showed an excellent dispersion over SiO2 support, featuring good catalytic activity in terms of hydrogenation of LA into GVL at a yield of 96% along with 4% Angelina lactone at 285 °C. The bimetallic Ni–Cu/SiO2 catalyst characterized good stability for prolonged runs of 200 h. This robustness is attributed to nanocomposite morphology nature of Cu–Si, which prevents metallic sintering. Indeed, the highest H2-uptake chemisorption of 0.039 mmol g−1 corresponds to the optimal catalyst loading of 20% Ni & 60% Cu–SiO2, which proved a homogeneous dispersion of metallic nanoparticles.99 In another study, doping Ni metal on RANEY® catalyst resulted in a complete conversion of LA (100%) and a yield of GVL at 68.5% using a ratio FA/LA of 4:1 under 200 °C for 48 h. The RANEY® Ni catalyst was able to catalyse cellulose under same conditions into GVL at yield 23.3%.111
Considering the synergetic relation between Cu & SiO2 and the improved catalytic activity obtained, Lomate S. et al. (2017)96 characterized the SiO2 supports and Cu-doped SiO2 catalysts, thereby studying the relation between the morphology and its activity. The physio-chemical properties of the catalyst were investigated and found to affect its activity. For instance, the highest TOF of 0.0707 moles LA h−1 g−1 corresponds to Cu–SiO2 catalyst with larger CuO clusters with stronger interaction with SiO2 surface. The strong interaction was also confirmed by the existence of the partial oxidation of Cu species represented as Cuδ+ with a binding energy 933.25 ± 0.35 eV located between Cu+ and Cu2+. Indeed, the higher activity of Cu–SiO2 catalyst was attributed to its morphology, having narrow pore diameter distribution that plays a role in confinement of smaller Cu clusters inside pore walls, thus easily accessible for LA hydrogenation into GVL. Indeed, this work has thoroughly investigated the complex role of acid nature of the catalyst surface and its redox properties have on its activity and product selectivity. The use of characterization tools provided solid details about the catalyst nature including its electronic structure, which facilitated drawing a conclusion that Lewis acid sites of medium acid strength played a key role in the conversion of LA into GVL. Whilst Brønsted acid sites provoked hydrogenolysis of GVL into further hydrocarbons over metal sites and thus, increasing the yield of pentanoic acid and angelica lactone (AL) on the expense of GVL. The presence of mononuclear Cu2+ over oligomeric (Cu–O–Cu)n+ led to higher activity of Cu/SiO2 catalyst at 66% LA conversion and 81% GVL yield (Fig. 8).96
Fig. 8 Conversion routes of LA into GVL.96 |
Designing a cost-effective route for hydrogenating LA into GVL using FA put it forward for considering the use of non-noble metal supported on oxides surfaces. For instance, ZnAl oxides were tested using different temperatures and LA/FA ratios, where it exhibited considerable GVL yield of 90% and LA conversion near 85% after 6 h reaction time at 140 °C and 5:1 FA/LA ratio.112 The work also featured kinetic modelling for proposed FA decomposition, LA hydrogenation as well as reversible formation of angelica lactone (AL) intermediates. The inhibitory effect of side reactions lies in the formation of lactones oligomers strongly adsorbed over basic sites of catalysts. Moreover, dehydrogenation of FA and hydrogenation of AL are key factors that establish the bounds within which LA dehydration reversible reaction is promoted in the forward direction without allowing the accumulation of intermediates (AL) (Fig. 8).112
From all the aforementioned information, LA can be transformed into its building blocks, which serve as valuable chemicals and biofuels additives. Together with GVL, LA can also be converted into other platform compounds such as pentanoic acid (valeric acid)57,113,114 or pentenoic acid115–118 (Fig. 3). In detail, GVL yielded from LA experiences ring opening to produce PA and pentanoic esters that undergo subsequent catalytic deoxygenating reactions to produce higher alkanes. As an illustration, Bond et al. established a dual catalytic system that comprises SiO2/Al2O3 followed by HZSM-5/Amberlyst acid catalysts, producing higher alkenes from butene and pentenoic acid intermediates.13,119 Likewise, pentanoic acid is also produced from GVL via hydrogenation/ring-opening before it experiences a consequent transformation into liquid alkanes, having distinctive properties which qualify it as a good diesel fuel blend.66 Lately, Zixiao Yi et al. introduced a comparative study of doping acidic catalyst by different metals; Ni and Ru. The two metals showed different reaction routes by which 3 wt% Ni/HZSM-5 catalyst resulted by limited hydrogenation of LA into GVL, whilst 3 wt% Ru/HZSM-5 catalyst facilitated further hydrogenation reaction, resulting in PA and pentanoic esters.120 Identically, the increase in acidic density due to Ru inclusion as well as 1.6 Pt MP−1-ZrO2 gave rise to PA production via GVL ring-opening mechanism.85 This comes in agreement with the findings of P. Sun et al. who reported that excessive acidity leads to decreasing GVL yields due to further ring opening reactions.117 Similarly, the dispersion of metal and the strong interaction between the metal and the doped acidic support MCM-49 can be adjusted by which a mesoporous Ru/MCM-49 can achieve LA conversion into GVL. This high conversion expressed by a TOF value of 3000 h−1 was attributed to the high amounts of lewis acid sites on which lactonization of 4-hydroxypentanoic acid into GVL is achieved.121 Metal active sites incorporated in heterogeneous catalysts experience some inhibitory factors that retard its activity, one of which is metal leaching due to the presence of the organic levulinic acid substrate. Interestingly, Bai X. et al. have developed a robust catalyst based on Ag–ZrO2–graphene oxide nanocomposite.122 In this perspective, Li J. et al. developed an attractive ternary catalyst Cu/ZrO2–Al2O3 for converting LA into GVL while avoiding the leaching of Cu. This was attributed to the existence of oxygen vacancies in the extra framework of the catalyst on which LA is adsorbed before it subsequently transforms into GVL.123 In the same context, it was reported that sol–gel entrapment of Ru in ZrO2 minimizes leaching of Ru/ZrO2 catalyst when used under acidic conditions (pH = 3.4). A conversion near 73% of LA and a complete decomposition of FA/HCOO− (100% conversion) were attained using only 2.5% wt Ru over ZrO2. Additionally, the authors tested the catalyst stability by incorporating 0.1 wt% SiO2, which eventually hindered any change of the tetragonal crystalline phase into monoclinic one.124
Generally speaking, designing non-noble metal-based catalysts has been an attractive material for researchers owing to its low cost and abundance that adds to the sustainability of the process. To demonstrate, Ni was one of the most used active metal species.91,125–127 With this in mind, Ni/NiO showed a quantitative LA conversion and GVL yield of 100% and 99.9%, respectively, at a relatively low temperature of 120 °C and 20 bar H2.126 Other research groups considered the acidity of catalyst support as a key factor in altering the conversion and yield of LA and GVL, respectively. In this context, acid supports, SiO2, Al2O3, Y–Al2O3 doped by Ni showed promising conversions of LA in the presence of external molecular H2.128–134 A complete conversion of LA and a GVL yield of 99.2% as well as a selectivity near 99.2% were exhibited using (40 wt%) Ni/Y–Al2O3 catalyst under dioxane solvent.132 In particular (15 wt%) Ni/Al2O3 showed high conversion without using a solvent.131 It is worth mentioning that active Ni species exist in the metallic state (Ni0), which comes in agreement with XPS results governing Ni0 (2p3/2) peaks,120 proving reduced catalyst improved activity.
Equally important, Cu non-noble metal is also doped on alumina and silica supports58,97,128,135 while other groups used zirconium oxide (ZrO2) supports.58,102,136 Amongst, Cu/SiO2 catalyzed intramolecular hydrogenation of LA by utilizing FA as an H2 donor with 28:22 wt% (LA:FA) ratio despite its low LA conversion of 48% and acceptable level of GVL selectivity of 80%.97 Nevertheless, Cu/ZrO2 catalyst outperformed Cu/SiO2 and achieved 60% LA conversion and 100% GVL selectivity by consuming FA. Furthermore, the former attained complete decomposition of LA at elevated temperatures of 200 °C for 5 h.102 Zirconium active species exist in both oxide states and Zr4+ on which LA hydrogenation takes place by using alcohol as solvents as well as H2 donor (2-propanol, 2-butanol, and 2-pentanol).94,95,137–141 The synergetic effect between Ni and Cu non-noble metals over SiO2 support was investigated in the vapour phase selective hydrogenation of LA into GVL using FA. The addition of Ni into Cu/SiO2 improved the hydrogenation of LA further compared to Cu/SiO2. The highest LA conversion of 99% and GVL selectivity of 96% was attributed to the optimal loading of 1:3 Ni to Cu at 285 °C. The temperature effect was demonstrated as both LA conversion and GVL selectivity increased with the increase of temperature. The good stability of the catalyst under high temperatures near Tamman temperature of Cu and for prolonged reactions up to 200 h was due to the presence of Ni. Interestingly, the excellent catalytic activity of nanocomposite was attributed to the excellent dispersion of the metallic nanoparticles and the absence of solid solution between Ni and Cu proved by the XRD and XPS.99
Based on the information mentioned above, two mechanisms characterize the hydrogenation of LA by means of in situ H2 donated by FA. The difference between the proposed mechanisms lies in different mode of adsorption of LA over the heterogeneous catalyst, resulting in a different intermediate compound. The first approach is outlined by forming 4-hydroxyvaleric acid intermediate as a result of LA hydrogenation over the metal active sites doped onto support. Thereafter, the 4-hydroxyvaleric acid undergoes dehydration step (lactonization) over acidic sites, for instance MP-ZrO2, to form GVL.85 Whereas the alternative route comprises the inverse order, where LA experiences dehydration step first over acidic sites to produce angelina lactone, which is readily hydrogenated into GVL over metal sites later.12,142,143 A conclusive table that sums the recent work in heterogeneous catalysis reported between 2017–2021 (Table 2).
Year | Substrate | H2 Donor | Catalyst | T (°C) | t (h) | Xa/Yb/TOFc | Recyclability | S% GVLd/ALe/VAf | Ref. |
---|---|---|---|---|---|---|---|---|---|
a X = conversion (%); Y = yield (%); TOF = turnover frequency (s−1) S = selectivity (%); LA = levulinic acid; GVL = γ-valerolactone; AL = angelica lactone; VA = valeric acid. | |||||||||
2017 | LA | FA | Cu–SiO2 | 230 | 1 | 53%a | 82%d | 96 | |
Cu–SiO2 | 270 | 1 | 66%a | 81%d | |||||
Cu–SiO2 | 290 | 1 | 68%a | 75%d | |||||
2017 | LA | FA | Triethoxy-silylpropoxy-Shvo's catalys | 90 | 12 | 90.93%a | 99.90%d | 70 | |
28c | |||||||||
2018 | LA | FA | Au–Ni/γ-Al2O3 | 190 | 2 | 89%a, 86%b | 83 | ||
2018 | LA | FA | 2 wt% Au/Ce0.4Zr0.6O2 | 240 | 2 | 90.8%a | • Recovery of catalyst by centrifugation, then washing with pure water and ethanol and dry at room temperature | 100%d | 82 |
83.5%b | |||||||||
Au/ZrO2 | 240 | 2 | 40.7%a | 89.5%d | |||||
36.4%b | |||||||||
0.6 wt% Au/Ce0.4Zr0.6O2 | 240 | 2 | 63.5%a | 77.3%d | |||||
49.7%b | |||||||||
240 | 2 | 13.1%a | • Good stability due to tetragonal phase attributing to strong metal–support interaction | 70.2%d | |||||
Au/CeO2 | 9.2%b | • Limited decrease in activity after 5 runs | |||||||
2018 | LA | FA | Calcined hydrotalcite Mg/Al (3:1) | 270 | 5 | 100%a | • Cycle I TOS = 30 h | 98%d | 101 |
1%e | |||||||||
Cycle II TOS = 22 h | |||||||||
Cycle III TOS = 14 h | |||||||||
Cycle IV TOS = 9 h | |||||||||
• Regeneration of active sites under flowing air after each cycle | |||||||||
• After cycle IV, LA conversion slightly decreased to 86% | |||||||||
• After cycle IV, GVL selectivity was constant at 98% | |||||||||
2018 | LA | FA (1:1) | RANEY® Ni catalyst | 200 | 24 | 52.6%a 20.4%b | 111 | ||
FA (1:1) | RANEY® Ni catalyst | 200 | 48 | 62.6%a | |||||
24.4%b | |||||||||
FA (1:2) | RANEY® Ni catalyst | 200 | 48 | 90.9%a | |||||
60.5%b | |||||||||
FA (1:4) | RANEY® Ni catalyst | 200 | 48 | 100%a | |||||
68.5%b | |||||||||
2018 | LA | FA | 0.2 g Ru/C + 3 mL triethyl-amine | 160 | 3 | 87.26%a | 71 | ||
80.75%b | |||||||||
2018 | LA | FA | 2.5% Ru/ZrO2 | 150 | 12 | 73%a | • Catalyst washed with water | >99%d | 124 |
2.5% Ru/ZrO2 (WI) | 150 | 12 | 63%a | • Activity significantly from 73% to 54% in the second run | >99%d | ||||
• XRD showed transformation from tetragonal to the thermodynamically stable monoclinic structure | |||||||||
2018 | LA | FA | Cu–SiO2 | 250 | 1 | 48%a | • Deactivation of Cu–SiO2 catalyst studied at 250 °C with LA:FA ratio = 1:2 | 80%d | 97 |
17%e | |||||||||
Cu–TiO2 | 250 | 1 | 8%a | • Consistent conversion of LA (48%) and selectivity of GVL | 25%d | ||||
55%e | |||||||||
Cu-ZSM-5 | 250 | 1 | 38%a | • Strong interaction between Cu with SiO2 support | 4%d | ||||
82%e | |||||||||
Cu–Al2O3 | 250 | 1 | 24%a | • Insignificant coke formation of Cu–SiO2 and Cu–TiO2 catalysts | 77%d | ||||
15%e | |||||||||
2019 | LA | FA | 6 wt% Au/ZrO2 | 210 | 5 | 93.3%a | • Catalyst washed by acetone 5 times and dried at 100 °C for 2 h | 91.1%d | |
85%b | • Stable after 3 cycles with 69% yield of GVL | ||||||||
Selectivity of catalyst was not affected | |||||||||
4 wt% Au/ZrO2 | 210 | 5 | 80.8%a | 87.1%d | 84 | ||||
70.4%b | |||||||||
1 wt% Au/ZrO2 | 210 | 5 | 13.6%a | 98.5%d | |||||
13.4%b | |||||||||
2019 | LA | FA | 1.6 Pt/MP-ZrO2 | 220 | 24 | 82%a | 85 | ||
84%b | |||||||||
1.5 Pt/MP-ZrO2 | 220 | 24 | 53%a | ||||||
52%b | |||||||||
2020 | LA | FA | CoOx | 230 | 20 | 37.3%a | • Mn2CoOx catalyst showed durable performance after 5 cycles | 85.2%d | |
10%f | |||||||||
2020 | LA | FA | MnOx | 230 | 20 | 76.7%a | • Conversion of LA fluctuated slightly around 60% from the 1st to the 5th cycle | 74.7%d | 109 |
12%f | |||||||||
Mn2Co0.1Ox | 230 | 20 | 78.9%a | • GVL yield fluctuated between 84% and 87% from the 1st to the 5th cycle | 76.7%d | ||||
11.8%f | |||||||||
Mn2Co0.1Ox+ 0.1 mol L−1 Na2SO4 | 230 | 20 | 83.4%a | • Selectivity of VA did not change dramatically from the 1st to the 5th cycle | 70%d | ||||
14.1%f | |||||||||
2020 | LA | FA | 1Au/ZrO2 | 240 | 1 | 66.7%a | • Recyclability of 1Au–2Ni/ZrO2 catalyst | 90.9%d | 77 |
73.4 %b | |||||||||
1Au–2Ni/ZrO2 | 240 | 1 | 87.9%a | • Spent catalyst was recovered by simple filtration | 98.7%d | ||||
89.1%b | |||||||||
0.5Au–2Ni/ZrO2 | 240 | 1 | 62.2%a | • Calcined at 300 °C for 4 h. & reduced in H2 flow at 300 °C for 1h | 98.4%d | ||||
63%b | |||||||||
2Ni/ZrO2 | 240 | 1 | 1.2%b | • GVL yield showed a slight decrease after 3 cycles | |||||
• Good recyclability of Au–Ni/ZrO2 | |||||||||
2021 | LA | FA | ZnAl oxide | 140 | <6 | 87%a | • Continuous but slight decrease in LA conversion during first 4 cycles | 90%d | 112 |
90%b | • LA is being directly or indirectly deposited on catalytic surface | ||||||||
• After 4th cycle, used catalyst was calcined at 600 °C, and TPO results were similar to the fresh catalyst | |||||||||
2021 | Glucose | FA | Ru/TiO2 | 190 | 2 | 38.98%a | 144 |
The challenging task of valorisation of renewable biomass into its constituents, for example biofuels, places emphasis on synthesizing heterogeneous catalysis. Ultimately, researchers aim at developing a heterogeneous catalytic system where the conversion of hemicellulose part of biomass into biofuels such as GVL in a one-pot process is achieved, while avoiding the use of liquid acid. It was reported elsewhere that a catalyst blend of ZSM-5 and Au/ZrO2 achieved a complete conversion of xylose and hemicellulose into furfural, followed by a subsequent hydrogenation into GVL at a yield of 80% in the presence of 2-propanol and without the need of external H2. The reaction was performed at 120 °C for 30 h which therefore resulted in a maintained a GVL yield not less than 65% after 4 reaction cycles of 24 h each.147
On another end, the use of heterogeneous catalysts facilitates its separation from the yielded product, and thereby the reuse of the catalyst is possible. Besides, heterogeneous catalysts suffer deactivation due to CO poisoning yielded by dehydration reaction37,38 due to elevated temperatures. For that reason, some research groups tended to manipulate the crystalline frameworks by calcination processes, which allow the synthesis of alloy, core–shell, and bimetallic structures. As shown above, an increase in Au cluster size due to thermal treatment decreased catalyst activity thereupon. Unfortunately, few studies were reported regarding the sintering effect on the active sites of heterogeneous catalysts as a result of elevated temperatures. Morphology and dispersion analysis of the active sites must be further performed using in situ SEM & TEM at different temperatures to inspect sintering and contamination deposition.
Coupled with its ability to accommodate massive energy content (5.3 MJ kg−1) as well as its low cost of production, making it an ideal fuel substitute, FA is a key compound for catalytic hydrogenation reactions. Specifically, FA is a key factor in LA hydrogenation into GVL, which undergoes successive deoxygenating reactions to yield higher alkanes (Section 3). In real applications, a pretreatment cracking step using strong acid (H2SO4, HCl) is carried out for lignocellulosic biomass and therefore heterogeneous catalysts are prone to deactivation. Different catalyst structures experience different effects of metal leaching on catalyst activity. For Cu catalysts, the leaching of metals detected through ICP-OES of the liquid products can lead to a significant reduction in catalyst activity down to 70%. Copper metal leaching was confirmed using FT-IR for investigating soluble copper complex.58 In other studies, ICP analysis showed that metals such as Fe, Ni, Cr, Co and Mo leach into the liquid product upon the hydrogenation of LA in the aqueous phase.6
Owing to the setback of metal leaching, designing a robust support is essential for improved metal–support interaction. Catalysts with carbon supports have been proved overcome the issue of leaching on the expense of catalyst regeneration.166 On the other hand, stable ZrO2 support of tetragonal phase demonstrated a stronger binding to the active Cu species (<2 ppm) than Al2O3 (174 ppm), avoiding metal leaching into the solvent.58
Further research should be employed on using either alternative acids20 or using conventional acids in appropriate quantities to avoid catalytic inhibition.66 Hence, it would be essential to perform LA catalytic hydrogenation by using FA as an H2 donor but under acidic conditions. Separating acids from the reaction mixture is a costly process. Alternatively, more attention should be given to solvents such as butene that yield immiscible levulinate esters.74 Findings achieved by Deng Li et al. suggested a promising effect of the addition of CO2 on the catalytic activity which should be investigated further as it exists as a major by-product as a result of FA dehydrogenation reaction.65 Likewise, studying the possibility of optimizing WGS reaction by injecting CO paves the road for utilizing the traces of CO existing in the product.167
Generally speaking, executing an optimized catalytic hydrogenation of LA through intramolecular H2 necessitates designing a catalytic reactor that accounts for engineering perspectives. Particularly, the assessment of heterogeneous catalysts must take into consideration heat and mass transfer as well as mass transfer limitations between the inner pore surface and the bulk biomass. That being said, designing different mixing systems is useful to obtain benchmark values of potential conversions range instead of just one conversion value for the studied catalyst. Furthermore, the produced gas could be continuously bubbled throughout the reactor in which better mixing and higher catalytic activity could be achieved. Equally important, further studies that integrate experimental results and simulations should be implemented, aiming to optimize reactor design and operating conditions. Continuous processes from engineering perspective are hardly found in literature and more efforts should be devoted to bringing pilot scale applications on table such as the work performed by Zhou et al.77 Scaling-up the process of production of valuable biomass-derived chemicals and biofuels from lignocellulosic derived LA requires considering its economic feasibility. A comprehensive techno-economic analysis performed by Patel A. et al. (2010) addresses the feasibility of producing 5-nonanone from LA and also evaluates the relative purification costs, both of which are based on discounted cash flow analysis.168 The model uses molecular H2 raw material input at 1736.07 kg h−1 of a market value 0.116 $ per kg. Indeed, shifting towards using stored H2 in FA disregards near 201 $ per h of the running cost of hydrogenation processes.168
All things considered, the most active heterogeneous catalysts comprise noble metals, which are expensive and less abundant in nature. However, some findings exhibited promising LA + FA conversion into GVL by using cheaper metals doped over acidic catalysts.120 Establishing less number of deoxygenating steps that yields valuable chemicals and/or higher liquid alkanes render them as a cost-effective catalytic route. In this regard, some developed catalysts85,120 produced higher alkanes bio-solvents beyond GVL despite the fact that they contain noble metals, putting a whole new set of development options on the table.
Footnote |
† Electronic supplementary information (ESI) available. See https://doi.org/10.1039/d2ra01379g |