Jun Jie Cao,
Yu Jiang,
Hang Zhan,
Yu Zhang* and
Jian Nong Wang*
School of Mechanical and Power Engineering, East China University of Science and Technology, 130 Meilong Road, Shanghai 200237, China. E-mail: jnwang@ecust.edu.cn; Tel: +86-21-64252360
First published on 5th December 2022
Vertically aligned carbon nanotubes (VACNTs), a unique group of highly aligned CNTs normal to a substrate, have been extensively studied during the past decades. However, it is a long-standing challenge to improve the height of VACNTs due to the incidental deactivation of catalysts during growth. Herein, we demonstrate a facile strategy toward synthesizing high-density and well-aligned CNT arrays from in situ formed Fe-based catalysts on a stainless steel (SS) mesh. These catalysts were generated by direct oxidation–reduction treatment to the SS, which had excellent adhesion on the mesh substrate, and thus suppressed catalyst aggregation and promoted CNT growth under the flow of C2H2. In particular, by feeding additional CO2 at an optimal rate, the height of CNT arrays could be boosted from ca. 15 μm to ca. 80.0 μm, one of the highest heights observed for VACNTs on SS-based substrates so far. This is attributed to the prolonged activity of the catalysts by CO2 induced removal of extra carbon. Our study might provide an insight into the development of efficient strategies for VACNT growth on conductive substrates.
Catalytic chemical vapor deposition (CCVD) has been one of the most commonly utilized approaches for preparing CNT arrays because of its simple operation, low cost, and relatively high growth efficiency.16 Up to date, VACNTs with millimeter-scale heights has been typically achieved by depositing catalysts on SiO2/Si substrates with an Al2O3 buffer layer.17 However, it is a tedious process to prepare the catalysts and then spray or sputter them on substrates. In addition, such VACNTs are subjected to limited applications due to the insulating or rigid properties of the substrates involved.
In recent years, using stainless steel (SS) as a conductive and flexible substrate has attracted some research.18–21 It has advantages of easy availability at low cost and high melting point (∼1300 °C), which enables the synthesis of CNTs at a wide temperature range. Furthermore, SS contains catalytic elements (e.g., Fe), making it possible to achieve direct CNT growth without additional buffer layers or catalysts.22 For example, Camilli et al. demonstrated the SS surface with a nanoscale roughness can act as the catalyst/template for the CNT growth via the chemical vapor deposition (CVD) method.23 Thapa et al. reported the direct synthesis of VACNTs (10.7 μm in height) on a SS substrate by using plasma enhanced CVD without external catalyst layers.24 Although such direct VACNT growth on SS has been reported, issues remain regarding the deactivation of the catalysts, too early termination of CNT growth, and thus the short heights of the CNT arrays. Previous studies also reported that the addition of CO2 or H2O worked as a weak oxidant to prolong the catalyst lifetime. For example, Yang et al. found that the CO2-assisted floating-ferrocene CVD method is favorable for the well-controlled growth of aligned CNT arrays. CNTs grown with CO2 addition were also higher than those grown in the absence of CO2, with the optimum CO2 concentration of 760 ppm producing a 50% enhancement in CNT height.25 Sato et al. compared the CO2-assisted CVD with the H2O-assisted one for VACNT growth, and found that equivalent structures and yields were obtained in these two cases.26 However, the underlying mechanism has not been investigated. In fact, it is highly desired to induce persistent growth of VACNTs on SS substrates with improved heights for practical applications.
In this study, we report an effective method for facile growth of high-density and well-aligned CNT arrays on a SS mesh. Efficient catalyst particles are in situ constructed after the direct oxidation and subsequent reduction treatment to the SS mesh. This is beneficial for preventing the aggregation of the catalyst particles due to their strong interaction with the substrate of high-melting point. When acetylene (C2H2) is used as a reactive carbon feedstock, highly-aligned CNT arrays are grown with high density on the pre-treated SS mesh at the temperature of 700 °C. In addition, CO2 is employed as an additive to boost the growth of VACNTs to high heights by etching the amorphous carbon on catalysts and thus prolonging their lifetime.
Fig. 1 Schematic illustrations of the experimental setup (a) and the process for the growth of VACNTS on SS mesh (b). |
Fig. 2a presents the optical image of the pristine SS mesh and VACNTs grown on the pre-treated SS (VACNTs/SS). It is noticed that the as-obtained VACNTs/SS became visibly black, suggesting the successful growth of VACNTs on the SS mesh. The low-magnification SEM image (Fig. 2b) further shows the coverage of VACNTs on the SS mesh, demonstrating the uniform distribution of catalytic sites. Fig. S3† shows the elemental mapping of VACNTs/SS. As shown in Fig. 2c, the CNT arrays were dense and well-aligned and the average height could be determined to be ca. 15 μm. The high-magnification SEM image (Fig. 2d) shows that these CNTs were curly and combined with each other, but still along the direction perpendicular to the substrate. Fig. 2e shows the X-ray diffraction patterns of the SS mesh before and after the VACNTs growth. The peaks located at 44°, 51°, and 75° recorded from the pristine SS mesh can be assigned to the (111), (200), and (220) planes of Fe metal (PDF No. 65-9094), respectively. In comparison, the intensity of those peaks for VACNTs/SS was significantly decreased, along with the emergence of one distinct peak at 25° corresponding to the (002) plane of CNTs. These observations suggest that the SS mesh was well covered by dense and tall VACNTs, leading to the reduced detection depth of substrates and thus decreased peak intensity. In addition, the XRD results of the as-oxidized SS mesh and oxidation–reduction treated SS are illustrated in Fig. S2.† The main components of the as-oxidized SS mesh and oxidation–reduction SS mesh were Fe2O3 and Fe, respectively. Fig. 2f shows the Raman spectrum of VACNTs with a high ratio (0.81) of ID (defect mediated D-band at ∼1350 cm−1) and IG (graphitic nature G-band at ∼1590 cm−1), indicating good structural quality of the as-prepared VACNTs.
The average diameter of CNTs was determined as ca. 13 nm (Fig. 3a) by statistical analysis from the low-magnification TEM image (Fig. 3b). The CNTs showed “bamboo-like” structures (Fig. 3c), which could be due to the dynamic changes of the catalyst particles in shape and size caused by the dissolution and precipitation of carbon atoms during the growth process. In addition, few catalyst particles were observed within or at the end cap of the CNTs, suggesting the base growth mode with catalysts anchored on the substrate during growth (Fig. S7†). This could be mainly due to the strong bonding of the in situ formed catalysts with the substrate by constructing chemical bonds during the oxidation–reduction process, which is favourable for preventing catalysts from migration and aggregation. In addition, the high-resolution TEM image demonstrates the multi-walled structure of the CNTs (Fig. 3d) with the clear d-spacing of 0.34 nm.
Fig. 3 (a) Diameter distribution of the VACNTs; (b–d) TEM images of CNTs obtained by sonicating VACNTs/SS in ethanol. |
Previous studies have demonstrated that the growth time played a key role in improving the length of CNTs.27–29 The present growth duration was extended from 30 min to 2 h with the expectation of further improving the height of VACNTs. Although the flow rate of C2H2 as the carbon precursor was as low as 10 sccm, a large number of particles (Fig. S4a and b†) appeared on the top of VACNTs after 2 h of growth. This observation suggests that the catalysts had been gradually deactivated, leading to the covering of carbon atoms on VACNTs instead of continuous growth.
In order to prolong the lifetime of the catalysts, CO2 was supplied as a weak oxidant by reacting with the carbon byproducts (e.g., amorphous carbon) on the surfaces of the catalysts.30–32 The CNT growth was performed at different CO2 flow rates of 10, 30, and 50 sccm, while other experimental conditions were kept to be the same. As shown in Fig. 4a, the height of VACNTs was improved from ∼10 μm to ∼35 μm compared with that of the sample prepared without CO2, demonstrating the significant effect of CO2 on boosting the CNT growth. However, when the flow rate of CO2 was increased to 30 sccm (Fig. 4b) and 50 sccm (Fig. 4c), the top layer of VACNTs became intertwined and the length was gradually reduced (Fig. 4d). This could be attributed to the lowered activities of the catalyst nanoparticles in the presence of too much CO2. At the optimal flow rate of CO2 of 10 sccm, the growth time was increased 30 min to 6 h. As a result, the VACNTs with a maximum height of 80 μm was obtained (Fig. 5a–d). This height appears to be the highest among the VACNTs prepared with the use of SS as the substrate (Table S2†).
Fig. 5 SEM images of VACNTs grown on SS with CO2 (10 sccm) in different growth durations: (a) 0.5 h; (b) 2 h; (c) 4 h; (d) 6 h. |
To explore the role of CO2 in CNT growth, the measurement of Raman spectroscopy was conducted for the samples obtained with or without CO2 feeding during the growth for 2 h. It was found that the ID/IG value of VACNTs decreased from 1.04 to 0.84 with CO2 feeding (Fig. 4e), suggesting the effect of CO2 on improving the graphitization degree of VACNTs. This could be mainly ascribed to that CO2 at an optimal flow rate can properly etch the amorphous carbon on CNTs by following the reaction of CO2 + C → 2CO. The schematic illustrating the mechanism involved in the presence/absence of CO2 is shown in Fig. S5.† However, CO2 at higher concentrations may not only react with amorphous carbon but also oxidize the Fe-based catalysts, leading to their deactivation and thus inhibition of the decomposition of C2H2. The XRD measurement of VACNT/SS to characterize the components upon CO2 treatment is illustrated in Fig. S6.† It can be found that the three main peaks locating at 43.72°, 50.94° and 74.94° correspond to diffractions of (111), (200), and (220) planes of Fe, respectively, while the other minor peak at 35.48° can be assigned to (400) plane of Fe3O4. These results confirmed our suggestion that the catalysts for CNT growth were mainly Fe after the oxidation–reduction process, and excessive CO2 could also react with Fe and form Fe-oxides (Fe3O4).
To further explore the mechanism of CO2 in prolonging the life time of the catalysts, gas chromatography was used to detect the concentrations of CO in the exhaust when different flow rates of CO2 were used. As shown in Fig. 4f, the concentration of CO gradually increased with increasing flow rate of CO2 (Fig. 4f and Table S1†), verifying the etching effect of CO2 by reacting with amorphous carbon.
In addition, we further used a larger SS mesh (2 cm × 50 cm) as the substrate to grow VACNTs with the purpose of verifying the possibility of scaling up using the same procedure. As shown in Fig. S8a,† the entire substrate was observed to be covered uniformly with black materials. We also observed the growth of VACNTs at different positions of the substrate (Fig. S8b–d†), thus demonstrating that our method holds potential for large-scale production of VACNTs.
Footnote |
† Electronic supplementary information (ESI) available. See DOI: https://doi.org/10.1039/d2ra04822a |
This journal is © The Royal Society of Chemistry 2022 |